Physical Properties | Original Value | Comments |
---|
Density | 7.65 g/cc |
Thickness | 200 - 240 microns |
| 230 microns |
|
Mechanical Properties | Original Value | Comments |
---|
Knoop Microhardness | 173 |
Hardness, Rockwell B | 83 |
Tensile Strength, Ultimate | 359 MPa |
Tensile Strength, Yield | 345 MPa |
Elongation at Break | 11 % |
Modulus of Elasticity | 113.8 GPa |
| 138 GPa |
| 203 GPa |
| 241 GPa |
| 276 GPa |
|
Electrical Properties | Original Value | Comments |
---|
Exciting Power (RMS) | 0.00290 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00290 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00360 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00370 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0100 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0101 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0126 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0128 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0208 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0209 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0263 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0264 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0342 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0344 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0434 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0436 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0498 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0504 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0632 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0640 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0672 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0684 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0856 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0866 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.0871 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0885 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1077 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.1105 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.1105 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.1127 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.1309 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.1345 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.1377 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.1414 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.1564 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.1609 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.1682 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.1723 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.1841 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.1895 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.2009 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.2064 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.2155 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.2218 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.2368 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.2436 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.2518 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.2582 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.2768 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.285 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.2909 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.300 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.3227 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.3314 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.3409 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.3536 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.3741 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.3855 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.4095 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.4291 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.4368 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.4527 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.5209 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.5459 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.5505 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.5632 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.6955 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.7077 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 0.9409 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 0.9545 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.1591 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.1818 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 3.8045 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 3.9409 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 4.65 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
| 4.8136 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000500 ohm-cm |
|
Magnetic Properties | Original Value | Comments |
---|
Core Loss | 0.00326 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00377 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00430 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00497 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0123 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.01337 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.01638 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.01781 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0272 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0289 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0363 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0385 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0476 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0499 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0634 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0665 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0731 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0761 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0972 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.1013 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.1035 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.1074 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.1374 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.1389 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1426 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.1435 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1792 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.1841 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.1847 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.1902 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.225 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.231 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.237 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.245 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.275 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.283 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.297 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.306 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.332 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.341 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.364 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.374 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.394 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.405 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.438 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.450 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.463 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.475 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.521 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.534 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.539 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.552 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.611 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.620 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.625 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.627 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.639 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.711 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.720 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.729 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.741 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.824 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.830 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.843 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.850 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.852 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.871 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz |
| <= 0.900 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.947 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.974 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz |
| 1.065 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.092 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.115 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.12 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.141 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz |
| <= 1.19 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.384 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.42 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.558 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz |
| 1.586 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz |
| 2.00 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz |
| 2.05 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Approximate Equivalent International Grade | M090-23P5 |
Magnetostriction 10^8 | -32 |
| -37 |
| -40 |
| -44 |
Maximum Induction at 800 A/m (T) | 1.88 |
Minimum Lamination Factor (%) | 94.5 |
Typical Induction at 800 A/m (T) | 1.917 |
Typical Lamination Factor (%) | 96.6 |