Physical Properties | Metric | English | Comments |
---|
Density | 7.65 g/cc | 0.276 lb/in³ |
Thickness | 250 microns | 9.84 mil |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell B | 78 | 78 |
Tensile Strength, Ultimate | 450 MPa | 65300 psi |
Tensile Strength, Yield | 350 MPa | 50800 psi |
Elongation at Break | 20 % | 20 % |
|
Electrical Properties | Metric | English | Comments |
---|
Exciting Power | 0.0188 VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz | 0.0188 VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.0226 VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz | 0.0226 VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0226 VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz | 0.0226 VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.0273 VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz | 0.0273 VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0385 VA/lb @Magnetic Field 0.100 T, Frequency 100 Hz | 0.0385 VA/lb @Magnetic Field 0.100 T, Frequency 100 Hz |
| 0.0459 VA/lb @Magnetic Field 0.100 T, Frequency 100 Hz | 0.0459 VA/lb @Magnetic Field 0.100 T, Frequency 100 Hz |
| 0.0536 VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0536 VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0650 VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0650 VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0650 VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0650 VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0786 VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0786 VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0800 VA/lb @Magnetic Field 0.100 T, Frequency 200 Hz | 0.0800 VA/lb @Magnetic Field 0.100 T, Frequency 200 Hz |
| 0.0941 VA/lb @Magnetic Field 0.100 T, Frequency 200 Hz | 0.0941 VA/lb @Magnetic Field 0.100 T, Frequency 200 Hz |
| 0.1118 VA/lb @Magnetic Field 0.200 T, Frequency 100 Hz | 0.1118 VA/lb @Magnetic Field 0.200 T, Frequency 100 Hz |
| 0.1336 VA/lb @Magnetic Field 0.200 T, Frequency 100 Hz | 0.1336 VA/lb @Magnetic Field 0.200 T, Frequency 100 Hz |
| 0.1464 VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz | 0.1464 VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.1714 VA/lb @Magnetic Field 0.100 T, Frequency 400 Hz | 0.1714 VA/lb @Magnetic Field 0.100 T, Frequency 400 Hz |
| 0.1768 VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz | 0.1768 VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.1773 VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz | 0.1773 VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.1968 VA/lb @Magnetic Field 0.100 T, Frequency 400 Hz | 0.1968 VA/lb @Magnetic Field 0.100 T, Frequency 400 Hz |
| 0.2141 VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz | 0.2141 VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.2373 VA/lb @Magnetic Field 0.200 T, Frequency 200 Hz | 0.2373 VA/lb @Magnetic Field 0.200 T, Frequency 200 Hz |
| 0.2805 VA/lb @Magnetic Field 0.200 T, Frequency 200 Hz | 0.2805 VA/lb @Magnetic Field 0.200 T, Frequency 200 Hz |
| 0.310 VA/lb @Magnetic Field 0.400 T, Frequency 100 Hz | 0.310 VA/lb @Magnetic Field 0.400 T, Frequency 100 Hz |
| 0.3273 VA/lb @Magnetic Field 0.100 T, Frequency 700 Hz | 0.3273 VA/lb @Magnetic Field 0.100 T, Frequency 700 Hz |
| 0.3386 VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz | 0.3386 VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.3677 VA/lb @Magnetic Field 0.100 T, Frequency 700 Hz | 0.3677 VA/lb @Magnetic Field 0.100 T, Frequency 700 Hz |
| 0.3686 VA/lb @Magnetic Field 0.400 T, Frequency 100 Hz | 0.3686 VA/lb @Magnetic Field 0.400 T, Frequency 100 Hz |
| 0.4114 VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz | 0.4114 VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.4123 VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz | 0.4123 VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.4455 VA/lb @Magnetic Field 0.100 T, Frequency 1000 Hz | 0.4455 VA/lb @Magnetic Field 0.100 T, Frequency 1000 Hz |
| 0.500 VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz | 0.500 VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.5318 VA/lb @Magnetic Field 0.200 T, Frequency 400 Hz | 0.5318 VA/lb @Magnetic Field 0.200 T, Frequency 400 Hz |
| 0.5636 VA/lb @Magnetic Field 0.100 T, Frequency 1000 Hz | 0.5636 VA/lb @Magnetic Field 0.100 T, Frequency 1000 Hz |
| 0.6091 VA/lb @Magnetic Field 0.200 T, Frequency 400 Hz | 0.6091 VA/lb @Magnetic Field 0.200 T, Frequency 400 Hz |
| 0.650 VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz | 0.650 VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.6818 VA/lb @Magnetic Field 0.400 T, Frequency 200 Hz | 0.6818 VA/lb @Magnetic Field 0.400 T, Frequency 200 Hz |
| 0.7273 VA/lb @Magnetic Field 0.700 T, Frequency 100 Hz | 0.7273 VA/lb @Magnetic Field 0.700 T, Frequency 100 Hz |
| 0.7909 VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz | 0.7909 VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.7955 VA/lb @Magnetic Field 0.400 T, Frequency 200 Hz | 0.7955 VA/lb @Magnetic Field 0.400 T, Frequency 200 Hz |
| 0.800 VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz | 0.800 VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.8636 VA/lb @Magnetic Field 0.700 T, Frequency 100 Hz | 0.8636 VA/lb @Magnetic Field 0.700 T, Frequency 100 Hz |
| 0.900 VA/lb @Magnetic Field 0.100 T, Frequency 1500 Hz | 0.900 VA/lb @Magnetic Field 0.100 T, Frequency 1500 Hz |
| 0.9364 VA/lb @Magnetic Field 0.100 T, Frequency 1500 Hz | 0.9364 VA/lb @Magnetic Field 0.100 T, Frequency 1500 Hz |
| 0.9682 VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz | 0.9682 VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 1.0636 VA/lb @Magnetic Field 0.200 T, Frequency 700 Hz | 1.0636 VA/lb @Magnetic Field 0.200 T, Frequency 700 Hz |
| 1.0773 VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz | 1.0773 VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 1.1909 VA/lb @Magnetic Field 0.200 T, Frequency 700 Hz | 1.1909 VA/lb @Magnetic Field 0.200 T, Frequency 700 Hz |
| 1.3045 VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz | 1.3045 VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 1.3364 VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz | 1.3364 VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 1.3864 VA/lb @Magnetic Field 1.00 T, Frequency 100 Hz | 1.3864 VA/lb @Magnetic Field 1.00 T, Frequency 100 Hz |
| 1.5591 VA/lb @Magnetic Field 0.200 T, Frequency 1000 Hz | 1.5591 VA/lb @Magnetic Field 0.200 T, Frequency 1000 Hz |
| 1.5864 VA/lb @Magnetic Field 0.400 T, Frequency 400 Hz | 1.5864 VA/lb @Magnetic Field 0.400 T, Frequency 400 Hz |
| 1.5864 VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz | 1.5864 VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 1.6136 VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz | 1.6136 VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 1.6318 VA/lb @Magnetic Field 0.700 T, Frequency 200 Hz | 1.6318 VA/lb @Magnetic Field 0.700 T, Frequency 200 Hz |
| 1.6682 VA/lb @Magnetic Field 1.00 T, Frequency 100 Hz | 1.6682 VA/lb @Magnetic Field 1.00 T, Frequency 100 Hz |
| 1.8045 VA/lb @Magnetic Field 0.400 T, Frequency 400 Hz | 1.8045 VA/lb @Magnetic Field 0.400 T, Frequency 400 Hz |
| 1.8591 VA/lb @Magnetic Field 0.100 T, Frequency 2500 Hz | 1.8591 VA/lb @Magnetic Field 0.100 T, Frequency 2500 Hz |
| 1.8818 VA/lb @Magnetic Field 0.200 T, Frequency 1000 Hz | 1.8818 VA/lb @Magnetic Field 0.200 T, Frequency 1000 Hz |
| 1.8909 VA/lb @Magnetic Field 0.700 T, Frequency 200 Hz | 1.8909 VA/lb @Magnetic Field 0.700 T, Frequency 200 Hz |
| 1.8955 VA/lb @Magnetic Field 0.100 T, Frequency 2500 Hz | 1.8955 VA/lb @Magnetic Field 0.100 T, Frequency 2500 Hz |
| 1.9273 VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz | 1.9273 VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 1.9591 VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz | 1.9591 VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 2.25 VA/lb @Magnetic Field 1.20 T, Frequency 100 Hz | 2.25 VA/lb @Magnetic Field 1.20 T, Frequency 100 Hz |
| 2.3636 VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz | 2.3636 VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 2.7545 VA/lb @Magnetic Field 1.20 T, Frequency 100 Hz | 2.7545 VA/lb @Magnetic Field 1.20 T, Frequency 100 Hz |
| 3.0727 VA/lb @Magnetic Field 0.200 T, Frequency 1500 Hz | 3.0727 VA/lb @Magnetic Field 0.200 T, Frequency 1500 Hz |
| 3.10 VA/lb @Magnetic Field 1.00 T, Frequency 200 Hz | 3.10 VA/lb @Magnetic Field 1.00 T, Frequency 200 Hz |
| 3.2364 VA/lb @Magnetic Field 0.200 T, Frequency 1500 Hz | 3.2364 VA/lb @Magnetic Field 0.200 T, Frequency 1500 Hz |
| 3.2864 VA/lb @Magnetic Field 1.30 T, Frequency 100 Hz | 3.2864 VA/lb @Magnetic Field 1.30 T, Frequency 100 Hz |
| 3.3409 VA/lb @Magnetic Field 0.400 T, Frequency 700 Hz | 3.3409 VA/lb @Magnetic Field 0.400 T, Frequency 700 Hz |
| 3.3455 VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz | 3.3455 VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 3.6273 VA/lb @Magnetic Field 1.00 T, Frequency 200 Hz | 3.6273 VA/lb @Magnetic Field 1.00 T, Frequency 200 Hz |
| 3.6682 VA/lb @Magnetic Field 0.400 T, Frequency 700 Hz | 3.6682 VA/lb @Magnetic Field 0.400 T, Frequency 700 Hz |
| 3.7818 VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz | 3.7818 VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 3.9318 VA/lb @Magnetic Field 0.700 T, Frequency 400 Hz | 3.9318 VA/lb @Magnetic Field 0.700 T, Frequency 400 Hz |
| 3.9955 VA/lb @Magnetic Field 1.30 T, Frequency 100 Hz | 3.9955 VA/lb @Magnetic Field 1.30 T, Frequency 100 Hz |
| 4.0636 VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz | 4.0636 VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 4.4182 VA/lb @Magnetic Field 0.700 T, Frequency 400 Hz | 4.4182 VA/lb @Magnetic Field 0.700 T, Frequency 400 Hz |
| 4.5455 VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz | 4.5455 VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 4.9091 VA/lb @Magnetic Field 1.20 T, Frequency 200 Hz | 4.9091 VA/lb @Magnetic Field 1.20 T, Frequency 200 Hz |
| 5.2273 VA/lb @Magnetic Field 0.400 T, Frequency 1000 Hz | 5.2273 VA/lb @Magnetic Field 0.400 T, Frequency 1000 Hz |
| 5.5455 VA/lb @Magnetic Field 0.100 T, Frequency 5000 Hz | 5.5455 VA/lb @Magnetic Field 0.100 T, Frequency 5000 Hz |
| 5.6818 VA/lb @Magnetic Field 0.100 T, Frequency 5000 Hz | 5.6818 VA/lb @Magnetic Field 0.100 T, Frequency 5000 Hz |
| 5.8636 VA/lb @Magnetic Field 1.20 T, Frequency 200 Hz | 5.8636 VA/lb @Magnetic Field 1.20 T, Frequency 200 Hz |
| 5.9545 VA/lb @Magnetic Field 0.400 T, Frequency 1000 Hz | 5.9545 VA/lb @Magnetic Field 0.400 T, Frequency 1000 Hz |
| 6.5909 VA/lb @Magnetic Field 0.200 T, Frequency 2500 Hz | 6.5909 VA/lb @Magnetic Field 0.200 T, Frequency 2500 Hz |
| 6.6818 VA/lb @Magnetic Field 0.200 T, Frequency 2500 Hz | 6.6818 VA/lb @Magnetic Field 0.200 T, Frequency 2500 Hz |
| 6.9091 VA/lb @Magnetic Field 1.40 T, Frequency 100 Hz | 6.9091 VA/lb @Magnetic Field 1.40 T, Frequency 100 Hz |
| 7.00 VA/lb @Magnetic Field 1.30 T, Frequency 200 Hz | 7.00 VA/lb @Magnetic Field 1.30 T, Frequency 200 Hz |
| 7.5455 VA/lb @Magnetic Field 1.00 T, Frequency 400 Hz | 7.5455 VA/lb @Magnetic Field 1.00 T, Frequency 400 Hz |
| 7.5909 VA/lb @Magnetic Field 1.40 T, Frequency 100 Hz | 7.5909 VA/lb @Magnetic Field 1.40 T, Frequency 100 Hz |
| 8.3182 VA/lb @Magnetic Field 1.30 T, Frequency 200 Hz | 8.3182 VA/lb @Magnetic Field 1.30 T, Frequency 200 Hz |
| 8.4545 VA/lb @Magnetic Field 1.00 T, Frequency 400 Hz | 8.4545 VA/lb @Magnetic Field 1.00 T, Frequency 400 Hz |
| 8.50 VA/lb @Magnetic Field 0.700 T, Frequency 700 Hz | 8.50 VA/lb @Magnetic Field 0.700 T, Frequency 700 Hz |
| 9.2727 VA/lb @Magnetic Field 0.700 T, Frequency 700 Hz | 9.2727 VA/lb @Magnetic Field 0.700 T, Frequency 700 Hz |
| 10.0909 VA/lb @Magnetic Field 0.400 T, Frequency 1500 Hz | 10.0909 VA/lb @Magnetic Field 0.400 T, Frequency 1500 Hz |
| 10.4545 VA/lb @Magnetic Field 0.400 T, Frequency 1500 Hz | 10.4545 VA/lb @Magnetic Field 0.400 T, Frequency 1500 Hz |
| 11.0 VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz | 11.0 VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 11.5909 VA/lb @Magnetic Field 1.20 T, Frequency 400 Hz | 11.5909 VA/lb @Magnetic Field 1.20 T, Frequency 400 Hz |
| 11.6364 VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz | 11.6364 VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 13.2273 VA/lb @Magnetic Field 1.20 T, Frequency 400 Hz | 13.2273 VA/lb @Magnetic Field 1.20 T, Frequency 400 Hz |
| 13.3636 VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz | 13.3636 VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 13.8182 VA/lb @Magnetic Field 0.700 T, Frequency 1000 Hz | 13.8182 VA/lb @Magnetic Field 0.700 T, Frequency 1000 Hz |
| 14.0909 VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz | 14.0909 VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 14.1364 VA/lb @Magnetic Field 1.40 T, Frequency 200 Hz | 14.1364 VA/lb @Magnetic Field 1.40 T, Frequency 200 Hz |
| 15.3636 VA/lb @Magnetic Field 0.700 T, Frequency 1000 Hz | 15.3636 VA/lb @Magnetic Field 0.700 T, Frequency 1000 Hz |
| 15.5 VA/lb @Magnetic Field 1.40 T, Frequency 200 Hz | 15.5 VA/lb @Magnetic Field 1.40 T, Frequency 200 Hz |
| 15.8182 VA/lb @Magnetic Field 1.30 T, Frequency 400 Hz | 15.8182 VA/lb @Magnetic Field 1.30 T, Frequency 400 Hz |
| 16.5909 VA/lb @Magnetic Field 1.00 T, Frequency 700 Hz | 16.5909 VA/lb @Magnetic Field 1.00 T, Frequency 700 Hz |
| 16.7273 VA/lb @Magnetic Field 0.100 T, Frequency 10000 Hz | 16.7273 VA/lb @Magnetic Field 0.100 T, Frequency 10000 Hz |
| 16.7727 VA/lb @Magnetic Field 0.100 T, Frequency 10000 Hz | 16.7727 VA/lb @Magnetic Field 0.100 T, Frequency 10000 Hz |
| 18.0455 VA/lb @Magnetic Field 1.00 T, Frequency 700 Hz | 18.0455 VA/lb @Magnetic Field 1.00 T, Frequency 700 Hz |
| 18.1364 VA/lb @Magnetic Field 1.30 T, Frequency 400 Hz | 18.1364 VA/lb @Magnetic Field 1.30 T, Frequency 400 Hz |
| 19.1818 VA/lb @Magnetic Field 0.200 T, Frequency 5000 Hz | 19.1818 VA/lb @Magnetic Field 0.200 T, Frequency 5000 Hz |
| 19.6364 VA/lb @Magnetic Field 0.200 T, Frequency 5000 Hz | 19.6364 VA/lb @Magnetic Field 0.200 T, Frequency 5000 Hz |
| 21.7273 VA/lb @Magnetic Field 0.400 T, Frequency 2500 Hz | 21.7273 VA/lb @Magnetic Field 0.400 T, Frequency 2500 Hz |
| 22.0 VA/lb @Magnetic Field 0.400 T, Frequency 2500 Hz | 22.0 VA/lb @Magnetic Field 0.400 T, Frequency 2500 Hz |
| 22.2727 VA/lb @Magnetic Field 1.50 T, Frequency 100 Hz | 22.2727 VA/lb @Magnetic Field 1.50 T, Frequency 100 Hz |
| 24.5455 VA/lb @Magnetic Field 1.50 T, Frequency 100 Hz | 24.5455 VA/lb @Magnetic Field 1.50 T, Frequency 100 Hz |
| 25.2727 VA/lb @Magnetic Field 1.20 T, Frequency 700 Hz | 25.2727 VA/lb @Magnetic Field 1.20 T, Frequency 700 Hz |
| 27.0 VA/lb @Magnetic Field 0.700 T, Frequency 1500 Hz | 27.0 VA/lb @Magnetic Field 0.700 T, Frequency 1500 Hz |
| 27.5455 VA/lb @Magnetic Field 1.00 T, Frequency 1000 Hz | 27.5455 VA/lb @Magnetic Field 1.00 T, Frequency 1000 Hz |
| 27.7273 VA/lb @Magnetic Field 0.700 T, Frequency 1500 Hz | 27.7273 VA/lb @Magnetic Field 0.700 T, Frequency 1500 Hz |
| 27.7273 VA/lb @Magnetic Field 1.20 T, Frequency 700 Hz | 27.7273 VA/lb @Magnetic Field 1.20 T, Frequency 700 Hz |
| 30.0455 VA/lb @Magnetic Field 1.40 T, Frequency 400 Hz | 30.0455 VA/lb @Magnetic Field 1.40 T, Frequency 400 Hz |
| 30.3182 VA/lb @Magnetic Field 1.00 T, Frequency 1000 Hz | 30.3182 VA/lb @Magnetic Field 1.00 T, Frequency 1000 Hz |
| 31.0 VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz | 31.0 VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 32.3636 VA/lb @Magnetic Field 1.40 T, Frequency 400 Hz | 32.3636 VA/lb @Magnetic Field 1.40 T, Frequency 400 Hz |
| 33.1818 VA/lb @Magnetic Field 1.30 T, Frequency 700 Hz | 33.1818 VA/lb @Magnetic Field 1.30 T, Frequency 700 Hz |
| 33.3636 VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz | 33.3636 VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 37.0455 VA/lb @Magnetic Field 1.30 T, Frequency 700 Hz | 37.0455 VA/lb @Magnetic Field 1.30 T, Frequency 700 Hz |
| 37.5 VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz | 37.5 VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 40.3636 VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz | 40.3636 VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 41.5 VA/lb @Magnetic Field 1.20 T, Frequency 1000 Hz | 41.5 VA/lb @Magnetic Field 1.20 T, Frequency 1000 Hz |
| 44.8182 VA/lb @Magnetic Field 1.50 T, Frequency 200 Hz | 44.8182 VA/lb @Magnetic Field 1.50 T, Frequency 200 Hz |
| 46.3636 VA/lb @Magnetic Field 1.20 T, Frequency 1000 Hz | 46.3636 VA/lb @Magnetic Field 1.20 T, Frequency 1000 Hz |
| 49.5455 VA/lb @Magnetic Field 1.50 T, Frequency 200 Hz | 49.5455 VA/lb @Magnetic Field 1.50 T, Frequency 200 Hz |
| 52.7273 VA/lb @Magnetic Field 1.30 T, Frequency 1000 Hz | 52.7273 VA/lb @Magnetic Field 1.30 T, Frequency 1000 Hz |
| 55.0 VA/lb @Magnetic Field 1.00 T, Frequency 1500 Hz | 55.0 VA/lb @Magnetic Field 1.00 T, Frequency 1500 Hz |
| 56.3636 VA/lb @Magnetic Field 1.00 T, Frequency 1500 Hz | 56.3636 VA/lb @Magnetic Field 1.00 T, Frequency 1500 Hz |
| 56.8182 VA/lb @Magnetic Field 0.200 T, Frequency 10000 Hz | 56.8182 VA/lb @Magnetic Field 0.200 T, Frequency 10000 Hz |
| 57.2727 VA/lb @Magnetic Field 0.200 T, Frequency 10000 Hz | 57.2727 VA/lb @Magnetic Field 0.200 T, Frequency 10000 Hz |
| 60.0 VA/lb @Magnetic Field 0.700 T, Frequency 2500 Hz | 60.0 VA/lb @Magnetic Field 0.700 T, Frequency 2500 Hz |
| 60.4545 VA/lb @Magnetic Field 1.30 T, Frequency 1000 Hz | 60.4545 VA/lb @Magnetic Field 1.30 T, Frequency 1000 Hz |
| 60.9091 VA/lb @Magnetic Field 0.700 T, Frequency 2500 Hz | 60.9091 VA/lb @Magnetic Field 0.700 T, Frequency 2500 Hz |
| 62.2727 VA/lb @Magnetic Field 1.60 T, Frequency 100 Hz | 62.2727 VA/lb @Magnetic Field 1.60 T, Frequency 100 Hz |
| 63.6364 VA/lb @Magnetic Field 0.400 T, Frequency 5000 Hz | 63.6364 VA/lb @Magnetic Field 0.400 T, Frequency 5000 Hz |
| 65.0 VA/lb @Magnetic Field 0.400 T, Frequency 5000 Hz | 65.0 VA/lb @Magnetic Field 0.400 T, Frequency 5000 Hz |
| 68.1818 VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz | 68.1818 VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 69.5455 VA/lb @Magnetic Field 1.60 T, Frequency 100 Hz | 69.5455 VA/lb @Magnetic Field 1.60 T, Frequency 100 Hz |
| 71.8182 VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz | 71.8182 VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 82.2727 VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz | 82.2727 VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 84.5455 VA/lb @Magnetic Field 1.20 T, Frequency 1500 Hz | 84.5455 VA/lb @Magnetic Field 1.20 T, Frequency 1500 Hz |
| 86.3636 VA/lb @Magnetic Field 1.20 T, Frequency 1500 Hz | 86.3636 VA/lb @Magnetic Field 1.20 T, Frequency 1500 Hz |
| 86.8182 VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz | 86.8182 VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 92.2727 VA/lb @Magnetic Field 1.50 T, Frequency 400 Hz | 92.2727 VA/lb @Magnetic Field 1.50 T, Frequency 400 Hz |
| 102.73 VA/lb @Magnetic Field 1.50 T, Frequency 400 Hz | 102.73 VA/lb @Magnetic Field 1.50 T, Frequency 400 Hz |
| 107.27 VA/lb @Magnetic Field 1.30 T, Frequency 1500 Hz | 107.27 VA/lb @Magnetic Field 1.30 T, Frequency 1500 Hz |
| 110 VA/lb @Magnetic Field 1.30 T, Frequency 1500 Hz | 110 VA/lb @Magnetic Field 1.30 T, Frequency 1500 Hz |
| 125.45 VA/lb @Magnetic Field 1.60 T, Frequency 200 Hz | 125.45 VA/lb @Magnetic Field 1.60 T, Frequency 200 Hz |
| 129.09 VA/lb @Magnetic Field 1.00 T, Frequency 2500 Hz | 129.09 VA/lb @Magnetic Field 1.00 T, Frequency 2500 Hz |
| 129.55 VA/lb @Magnetic Field 1.00 T, Frequency 2500 Hz | 129.55 VA/lb @Magnetic Field 1.00 T, Frequency 2500 Hz |
| 136.86 VA/lb @Magnetic Field 1.70 T, Frequency 100 Hz | 136.86 VA/lb @Magnetic Field 1.70 T, Frequency 100 Hz |
| 139.55 VA/lb @Magnetic Field 1.60 T, Frequency 200 Hz | 139.55 VA/lb @Magnetic Field 1.60 T, Frequency 200 Hz |
| 148.18 VA/lb @Magnetic Field 1.70 T, Frequency 100 Hz | 148.18 VA/lb @Magnetic Field 1.70 T, Frequency 100 Hz |
| 189.09 VA/lb @Magnetic Field 0.700 T, Frequency 5000 Hz | 189.09 VA/lb @Magnetic Field 0.700 T, Frequency 5000 Hz |
| 193.18 VA/lb @Magnetic Field 0.700 T, Frequency 5000 Hz | 193.18 VA/lb @Magnetic Field 0.700 T, Frequency 5000 Hz |
| 195 VA/lb @Magnetic Field 0.400 T, Frequency 10000 Hz | 195 VA/lb @Magnetic Field 0.400 T, Frequency 10000 Hz |
| 196.36 VA/lb @Magnetic Field 0.400 T, Frequency 10000 Hz | 196.36 VA/lb @Magnetic Field 0.400 T, Frequency 10000 Hz |
| 201.82 VA/lb @Magnetic Field 1.20 T, Frequency 2500 Hz | 201.82 VA/lb @Magnetic Field 1.20 T, Frequency 2500 Hz |
| 254.09 VA/lb @Magnetic Field 1.30 T, Frequency 2500 Hz | 254.09 VA/lb @Magnetic Field 1.30 T, Frequency 2500 Hz |
| 260.91 VA/lb @Magnetic Field 1.60 T, Frequency 400 Hz | 260.91 VA/lb @Magnetic Field 1.60 T, Frequency 400 Hz |
| 274.55 VA/lb @Magnetic Field 1.70 T, Frequency 200 Hz | 274.55 VA/lb @Magnetic Field 1.70 T, Frequency 200 Hz |
| 289.09 VA/lb @Magnetic Field 1.60 T, Frequency 400 Hz | 289.09 VA/lb @Magnetic Field 1.60 T, Frequency 400 Hz |
| 297.27 VA/lb @Magnetic Field 1.70 T, Frequency 200 Hz | 297.27 VA/lb @Magnetic Field 1.70 T, Frequency 200 Hz |
| 434.55 VA/lb @Magnetic Field 1.00 T, Frequency 5000 Hz | 434.55 VA/lb @Magnetic Field 1.00 T, Frequency 5000 Hz |
| 438.64 VA/lb @Magnetic Field 1.00 T, Frequency 5000 Hz | 438.64 VA/lb @Magnetic Field 1.00 T, Frequency 5000 Hz |
Electrical Resistivity | 0.0000540 - 0.0000560 ohm-cm | 0.0000540 - 0.0000560 ohm-cm |
|
Magnetic Properties | Metric | English | Comments |
---|
Core Loss | 0.0123 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00558 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.0125 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz | 0.00567 W/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.0151 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00685 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0153 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz | 0.00694 W/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.0271 W/kg @Magnetic Field 0.100 T, Frequency 100 Hz | 0.0123 W/lb @Magnetic Field 0.100 T, Frequency 100 Hz |
| 0.0279 W/kg @Magnetic Field 0.100 T, Frequency 100 Hz | 0.0127 W/lb @Magnetic Field 0.100 T, Frequency 100 Hz |
| 0.0498 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0226 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0556 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz | 0.0252 W/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0613 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0278 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0648 W/kg @Magnetic Field 0.100 T, Frequency 200 Hz | 0.0294 W/lb @Magnetic Field 0.100 T, Frequency 200 Hz |
| 0.0671 W/kg @Magnetic Field 0.100 T, Frequency 200 Hz | 0.0304 W/lb @Magnetic Field 0.100 T, Frequency 200 Hz |
| 0.0683 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz | 0.0310 W/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.112 W/kg @Magnetic Field 0.200 T, Frequency 100 Hz | 0.0508 W/lb @Magnetic Field 0.200 T, Frequency 100 Hz |
| 0.123 W/kg @Magnetic Field 0.200 T, Frequency 100 Hz | 0.0558 W/lb @Magnetic Field 0.200 T, Frequency 100 Hz |
| 0.170 W/kg @Magnetic Field 0.100 T, Frequency 400 Hz | 0.0771 W/lb @Magnetic Field 0.100 T, Frequency 400 Hz |
| 0.177 W/kg @Magnetic Field 0.100 T, Frequency 400 Hz | 0.0803 W/lb @Magnetic Field 0.100 T, Frequency 400 Hz |
| 0.179 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0812 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.205 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz | 0.0930 W/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.221 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.100 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.252 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz | 0.114 W/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.269 W/kg @Magnetic Field 0.200 T, Frequency 200 Hz | 0.122 W/lb @Magnetic Field 0.200 T, Frequency 200 Hz |
| 0.289 W/kg @Magnetic Field 0.200 T, Frequency 200 Hz | 0.131 W/lb @Magnetic Field 0.200 T, Frequency 200 Hz |
| 0.396 W/kg @Magnetic Field 0.100 T, Frequency 700 Hz | 0.180 W/lb @Magnetic Field 0.100 T, Frequency 700 Hz |
| 0.409 W/kg @Magnetic Field 0.400 T, Frequency 100 Hz | 0.186 W/lb @Magnetic Field 0.400 T, Frequency 100 Hz |
| 0.415 W/kg @Magnetic Field 0.100 T, Frequency 700 Hz | 0.188 W/lb @Magnetic Field 0.100 T, Frequency 700 Hz |
| 0.460 W/kg @Magnetic Field 0.400 T, Frequency 100 Hz | 0.209 W/lb @Magnetic Field 0.400 T, Frequency 100 Hz |
| 0.467 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.212 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.528 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz | 0.239 W/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.578 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.262 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.651 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz | 0.295 W/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.699 W/kg @Magnetic Field 0.100 T, Frequency 1000 Hz | 0.317 W/lb @Magnetic Field 0.100 T, Frequency 1000 Hz |
| 0.703 W/kg @Magnetic Field 0.200 T, Frequency 400 Hz | 0.319 W/lb @Magnetic Field 0.200 T, Frequency 400 Hz |
| 0.730 W/kg @Magnetic Field 0.100 T, Frequency 1000 Hz | 0.331 W/lb @Magnetic Field 0.100 T, Frequency 1000 Hz |
| 0.736 W/kg @Magnetic Field 0.200 T, Frequency 400 Hz | 0.334 W/lb @Magnetic Field 0.200 T, Frequency 400 Hz |
| 0.873 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.396 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.972 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz | 0.441 W/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.994 W/kg @Magnetic Field 0.400 T, Frequency 200 Hz | 0.451 W/lb @Magnetic Field 0.400 T, Frequency 200 Hz |
| 1.08 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.490 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 1.09 W/kg @Magnetic Field 0.400 T, Frequency 200 Hz | 0.494 W/lb @Magnetic Field 0.400 T, Frequency 200 Hz |
| 1.09 W/kg @Magnetic Field 0.700 T, Frequency 100 Hz | 0.494 W/lb @Magnetic Field 0.700 T, Frequency 100 Hz |
| 1.20 W/kg @Magnetic Field 0.700 T, Frequency 100 Hz | 0.544 W/lb @Magnetic Field 0.700 T, Frequency 100 Hz |
| 1.20 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz | 0.544 W/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 1.26 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.572 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 1.36 W/kg @Magnetic Field 0.100 T, Frequency 1500 Hz | 0.617 W/lb @Magnetic Field 0.100 T, Frequency 1500 Hz |
| 1.38 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz | 0.626 W/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 1.41 W/kg @Magnetic Field 0.100 T, Frequency 1500 Hz | 0.640 W/lb @Magnetic Field 0.100 T, Frequency 1500 Hz |
| 1.54 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.699 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 1.57 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.712 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 1.62 W/kg @Magnetic Field 0.200 T, Frequency 700 Hz | 0.735 W/lb @Magnetic Field 0.200 T, Frequency 700 Hz |
| 1.66 W/kg @Magnetic Field 0.200 T, Frequency 700 Hz | 0.753 W/lb @Magnetic Field 0.200 T, Frequency 700 Hz |
| 1.66 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz | 0.753 W/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 1.71 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz | 0.776 W/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 1.91 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.866 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 1.93 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.875 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 2.02 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz | 0.916 W/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 2.04 W/kg @Magnetic Field 1.00 T, Frequency 100 Hz | 0.925 W/lb @Magnetic Field 1.00 T, Frequency 100 Hz |
| 2.05 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz | 0.930 W/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 2.22 W/kg @Magnetic Field 1.00 T, Frequency 100 Hz | 1.01 W/lb @Magnetic Field 1.00 T, Frequency 100 Hz |
| 2.39 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 1.08 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 2.42 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 1.10 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 2.45 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz | 1.11 W/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 2.49 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz | 1.13 W/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 2.60 W/kg @Magnetic Field 0.400 T, Frequency 400 Hz | 1.18 W/lb @Magnetic Field 0.400 T, Frequency 400 Hz |
| 2.69 W/kg @Magnetic Field 0.700 T, Frequency 200 Hz | 1.22 W/lb @Magnetic Field 0.700 T, Frequency 200 Hz |
| 2.78 W/kg @Magnetic Field 0.400 T, Frequency 400 Hz | 1.26 W/lb @Magnetic Field 0.400 T, Frequency 400 Hz |
| 2.82 W/kg @Magnetic Field 0.200 T, Frequency 1000 Hz | 1.28 W/lb @Magnetic Field 0.200 T, Frequency 1000 Hz |
| 2.86 W/kg @Magnetic Field 0.200 T, Frequency 1000 Hz | 1.30 W/lb @Magnetic Field 0.200 T, Frequency 1000 Hz |
| 2.87 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 1.30 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 2.88 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz | 1.31 W/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 2.91 W/kg @Magnetic Field 0.700 T, Frequency 200 Hz | 1.32 W/lb @Magnetic Field 0.700 T, Frequency 200 Hz |
| 2.94 W/kg @Magnetic Field 1.20 T, Frequency 100 Hz | 1.33 W/lb @Magnetic Field 1.20 T, Frequency 100 Hz |
| 2.99 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 1.36 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 3.03 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz | 1.37 W/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 3.16 W/kg @Magnetic Field 1.20 T, Frequency 100 Hz | 1.43 W/lb @Magnetic Field 1.20 T, Frequency 100 Hz |
| 3.23 W/kg @Magnetic Field 0.100 T, Frequency 2500 Hz | 1.47 W/lb @Magnetic Field 0.100 T, Frequency 2500 Hz |
| 3.25 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 1.47 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 3.28 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz | 1.49 W/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 3.32 W/kg @Magnetic Field 0.100 T, Frequency 2500 Hz | 1.51 W/lb @Magnetic Field 0.100 T, Frequency 2500 Hz |
| 3.54 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 1.61 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 3.56 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz | 1.61 W/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 3.58 W/kg @Magnetic Field 1.30 T, Frequency 100 Hz | 1.62 W/lb @Magnetic Field 1.30 T, Frequency 100 Hz |
| 3.78 W/kg @Magnetic Field 1.30 T, Frequency 100 Hz | 1.71 W/lb @Magnetic Field 1.30 T, Frequency 100 Hz |
| 4.00 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 1.81 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 4.05 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz | 1.84 W/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 4.46 W/kg @Magnetic Field 1.40 T, Frequency 100 Hz | 2.02 W/lb @Magnetic Field 1.40 T, Frequency 100 Hz |
| 4.58 W/kg @Magnetic Field 1.40 T, Frequency 100 Hz | 2.08 W/lb @Magnetic Field 1.40 T, Frequency 100 Hz |
| 5.09 W/kg @Magnetic Field 1.00 T, Frequency 200 Hz | 2.31 W/lb @Magnetic Field 1.00 T, Frequency 200 Hz |
| 5.38 W/kg @Magnetic Field 0.200 T, Frequency 1500 Hz | 2.44 W/lb @Magnetic Field 0.200 T, Frequency 1500 Hz |
| 5.43 W/kg @Magnetic Field 0.200 T, Frequency 1500 Hz | 2.46 W/lb @Magnetic Field 0.200 T, Frequency 1500 Hz |
| 5.43 W/kg @Magnetic Field 1.00 T, Frequency 200 Hz | 2.46 W/lb @Magnetic Field 1.00 T, Frequency 200 Hz |
| 5.53 W/kg @Magnetic Field 1.50 T, Frequency 100 Hz | 2.51 W/lb @Magnetic Field 1.50 T, Frequency 100 Hz |
| 5.57 W/kg @Magnetic Field 1.50 T, Frequency 100 Hz | 2.53 W/lb @Magnetic Field 1.50 T, Frequency 100 Hz |
| 5.96 W/kg @Magnetic Field 0.400 T, Frequency 700 Hz | 2.70 W/lb @Magnetic Field 0.400 T, Frequency 700 Hz |
| 6.23 W/kg @Magnetic Field 0.400 T, Frequency 700 Hz | 2.83 W/lb @Magnetic Field 0.400 T, Frequency 700 Hz |
| 6.47 W/kg @Magnetic Field 1.60 T, Frequency 100 Hz | 2.93 W/lb @Magnetic Field 1.60 T, Frequency 100 Hz |
| 6.67 W/kg @Magnetic Field 1.60 T, Frequency 100 Hz | 3.03 W/lb @Magnetic Field 1.60 T, Frequency 100 Hz |
| 7.14 W/kg @Magnetic Field 0.700 T, Frequency 400 Hz | 3.24 W/lb @Magnetic Field 0.700 T, Frequency 400 Hz |
| 7.23 W/kg @Magnetic Field 1.70 T, Frequency 100 Hz | 3.28 W/lb @Magnetic Field 1.70 T, Frequency 100 Hz |
| 7.30 W/kg @Magnetic Field 1.20 T, Frequency 200 Hz | 3.31 W/lb @Magnetic Field 1.20 T, Frequency 200 Hz |
| 7.47 W/kg @Magnetic Field 1.70 T, Frequency 100 Hz | 3.39 W/lb @Magnetic Field 1.70 T, Frequency 100 Hz |
| 7.55 W/kg @Magnetic Field 0.700 T, Frequency 400 Hz | 3.42 W/lb @Magnetic Field 0.700 T, Frequency 400 Hz |
| 7.70 W/kg @Magnetic Field 1.20 T, Frequency 200 Hz | 3.49 W/lb @Magnetic Field 1.20 T, Frequency 200 Hz |
| 8.83 W/kg @Magnetic Field 1.30 T, Frequency 200 Hz | 4.01 W/lb @Magnetic Field 1.30 T, Frequency 200 Hz |
| 9.18 W/kg @Magnetic Field 1.30 T, Frequency 200 Hz | 4.16 W/lb @Magnetic Field 1.30 T, Frequency 200 Hz |
| 10.3 W/kg @Magnetic Field 0.400 T, Frequency 1000 Hz | 4.67 W/lb @Magnetic Field 0.400 T, Frequency 1000 Hz |
| 10.4 W/kg @Magnetic Field 0.100 T, Frequency 5000 Hz | 4.72 W/lb @Magnetic Field 0.100 T, Frequency 5000 Hz |
| 10.6 W/kg @Magnetic Field 0.400 T, Frequency 1000 Hz | 4.81 W/lb @Magnetic Field 0.400 T, Frequency 1000 Hz |
| 10.6 W/kg @Magnetic Field 0.100 T, Frequency 5000 Hz | 4.81 W/lb @Magnetic Field 0.100 T, Frequency 5000 Hz |
| 10.9 W/kg @Magnetic Field 1.40 T, Frequency 200 Hz | 4.94 W/lb @Magnetic Field 1.40 T, Frequency 200 Hz |
| 11.1 W/kg @Magnetic Field 1.40 T, Frequency 200 Hz | 5.03 W/lb @Magnetic Field 1.40 T, Frequency 200 Hz |
| 12.3 W/kg @Magnetic Field 0.200 T, Frequency 2500 Hz | 5.58 W/lb @Magnetic Field 0.200 T, Frequency 2500 Hz |
| 12.4 W/kg @Magnetic Field 0.200 T, Frequency 2500 Hz | 5.62 W/lb @Magnetic Field 0.200 T, Frequency 2500 Hz |
| 13.3 W/kg @Magnetic Field 1.50 T, Frequency 200 Hz | 6.03 W/lb @Magnetic Field 1.50 T, Frequency 200 Hz |
| 13.5 W/kg @Magnetic Field 1.50 T, Frequency 200 Hz | 6.12 W/lb @Magnetic Field 1.50 T, Frequency 200 Hz |
| 13.7 W/kg @Magnetic Field 1.00 T, Frequency 400 Hz | 6.21 W/lb @Magnetic Field 1.00 T, Frequency 400 Hz |
| 13.7 W/kg @Magnetic Field 1.00 T, Frequency 400 Hz | 6.21 W/lb @Magnetic Field 1.00 T, Frequency 400 Hz |
| 14.4 W/kg @Magnetic Field 1.00 T, Frequency 400 Hz | 6.53 W/lb @Magnetic Field 1.00 T, Frequency 400 Hz |
| 14.5 W/kg @Magnetic Field 1.00 T, Frequency 400 Hz | 6.58 W/lb @Magnetic Field 1.00 T, Frequency 400 Hz |
| <= 14.5 W/kg @Magnetic Field 1.00 T, Frequency 400 Hz | <= 6.58 W/lb @Magnetic Field 1.00 T, Frequency 400 Hz |
| 15.5 W/kg @Magnetic Field 1.60 T, Frequency 200 Hz | 7.03 W/lb @Magnetic Field 1.60 T, Frequency 200 Hz |
| 15.5 W/kg @Magnetic Field 1.00 T, Frequency 400 Hz | 7.03 W/lb @Magnetic Field 1.00 T, Frequency 400 Hz |
| 16.0 W/kg @Magnetic Field 1.60 T, Frequency 200 Hz | 7.26 W/lb @Magnetic Field 1.60 T, Frequency 200 Hz |
| 16.5 W/kg @Magnetic Field 0.700 T, Frequency 700 Hz | 7.48 W/lb @Magnetic Field 0.700 T, Frequency 700 Hz |
| 17.1 W/kg @Magnetic Field 0.700 T, Frequency 700 Hz | 7.76 W/lb @Magnetic Field 0.700 T, Frequency 700 Hz |
| 17.1 W/kg @Magnetic Field 1.70 T, Frequency 200 Hz | 7.76 W/lb @Magnetic Field 1.70 T, Frequency 200 Hz |
| 17.7 W/kg @Magnetic Field 1.70 T, Frequency 200 Hz | 8.03 W/lb @Magnetic Field 1.70 T, Frequency 200 Hz |
| 19.4 W/kg @Magnetic Field 0.400 T, Frequency 1500 Hz | 8.80 W/lb @Magnetic Field 0.400 T, Frequency 1500 Hz |
| 19.8 W/kg @Magnetic Field 0.400 T, Frequency 1500 Hz | 8.98 W/lb @Magnetic Field 0.400 T, Frequency 1500 Hz |
| 19.8 W/kg @Magnetic Field 1.20 T, Frequency 400 Hz | 8.98 W/lb @Magnetic Field 1.20 T, Frequency 400 Hz |
| 20.4 W/kg @Magnetic Field 1.20 T, Frequency 400 Hz | 9.25 W/lb @Magnetic Field 1.20 T, Frequency 400 Hz |
| 23.7 W/kg @Magnetic Field 1.30 T, Frequency 400 Hz | 10.8 W/lb @Magnetic Field 1.30 T, Frequency 400 Hz |
| 24.3 W/kg @Magnetic Field 1.30 T, Frequency 400 Hz | 11.0 W/lb @Magnetic Field 1.30 T, Frequency 400 Hz |
| 28.4 W/kg @Magnetic Field 0.700 T, Frequency 1000 Hz | 12.9 W/lb @Magnetic Field 0.700 T, Frequency 1000 Hz |
| 29.0 W/kg @Magnetic Field 1.40 T, Frequency 400 Hz | 13.2 W/lb @Magnetic Field 1.40 T, Frequency 400 Hz |
| 29.0 W/kg @Magnetic Field 1.40 T, Frequency 400 Hz | 13.2 W/lb @Magnetic Field 1.40 T, Frequency 400 Hz |
| 29.4 W/kg @Magnetic Field 0.700 T, Frequency 1000 Hz | 13.3 W/lb @Magnetic Field 0.700 T, Frequency 1000 Hz |
| 32.3 W/kg @Magnetic Field 1.00 T, Frequency 700 Hz | 14.7 W/lb @Magnetic Field 1.00 T, Frequency 700 Hz |
| 32.7 W/kg @Magnetic Field 0.100 T, Frequency 10000 Hz | 14.8 W/lb @Magnetic Field 0.100 T, Frequency 10000 Hz |
| 33.4 W/kg @Magnetic Field 1.00 T, Frequency 700 Hz | 15.1 W/lb @Magnetic Field 1.00 T, Frequency 700 Hz |
| 33.5 W/kg @Magnetic Field 0.100 T, Frequency 10000 Hz | 15.2 W/lb @Magnetic Field 0.100 T, Frequency 10000 Hz |
| 35.0 W/kg @Magnetic Field 1.50 T, Frequency 400 Hz | 15.9 W/lb @Magnetic Field 1.50 T, Frequency 400 Hz |
| 35.7 W/kg @Magnetic Field 1.50 T, Frequency 400 Hz | 16.2 W/lb @Magnetic Field 1.50 T, Frequency 400 Hz |
| 37.5 W/kg @Magnetic Field 0.200 T, Frequency 5000 Hz | 17.0 W/lb @Magnetic Field 0.200 T, Frequency 5000 Hz |
| 37.9 W/kg @Magnetic Field 0.200 T, Frequency 5000 Hz | 17.2 W/lb @Magnetic Field 0.200 T, Frequency 5000 Hz |
| 40.1 W/kg @Magnetic Field 1.60 T, Frequency 400 Hz | 18.2 W/lb @Magnetic Field 1.60 T, Frequency 400 Hz |
| 41.3 W/kg @Magnetic Field 1.60 T, Frequency 400 Hz | 18.7 W/lb @Magnetic Field 1.60 T, Frequency 400 Hz |
| 43.0 W/kg @Magnetic Field 0.400 T, Frequency 2500 Hz | 19.5 W/lb @Magnetic Field 0.400 T, Frequency 2500 Hz |
| 43.8 W/kg @Magnetic Field 0.400 T, Frequency 2500 Hz | 19.9 W/lb @Magnetic Field 0.400 T, Frequency 2500 Hz |
| 47.3 W/kg @Magnetic Field 1.20 T, Frequency 700 Hz | 21.5 W/lb @Magnetic Field 1.20 T, Frequency 700 Hz |
| 48.3 W/kg @Magnetic Field 1.20 T, Frequency 700 Hz | 21.9 W/lb @Magnetic Field 1.20 T, Frequency 700 Hz |
| 53.3 W/kg @Magnetic Field 0.700 T, Frequency 1500 Hz | 24.2 W/lb @Magnetic Field 0.700 T, Frequency 1500 Hz |
| 55.3 W/kg @Magnetic Field 0.700 T, Frequency 1500 Hz | 25.1 W/lb @Magnetic Field 0.700 T, Frequency 1500 Hz |
| 56.7 W/kg @Magnetic Field 1.00 T, Frequency 1000 Hz | 25.7 W/lb @Magnetic Field 1.00 T, Frequency 1000 Hz |
| 56.7 W/kg @Magnetic Field 1.30 T, Frequency 700 Hz | 25.7 W/lb @Magnetic Field 1.30 T, Frequency 700 Hz |
| 56.9 W/kg @Magnetic Field 1.30 T, Frequency 700 Hz | 25.8 W/lb @Magnetic Field 1.30 T, Frequency 700 Hz |
| 58.3 W/kg @Magnetic Field 1.00 T, Frequency 1000 Hz | 26.4 W/lb @Magnetic Field 1.00 T, Frequency 1000 Hz |
| 84.1 W/kg @Magnetic Field 1.20 T, Frequency 1000 Hz | 38.1 W/lb @Magnetic Field 1.20 T, Frequency 1000 Hz |
| 85.2 W/kg @Magnetic Field 1.20 T, Frequency 1000 Hz | 38.6 W/lb @Magnetic Field 1.20 T, Frequency 1000 Hz |
| 101.1 W/kg @Magnetic Field 1.30 T, Frequency 1000 Hz | 45.86 W/lb @Magnetic Field 1.30 T, Frequency 1000 Hz |
| 102 W/kg @Magnetic Field 1.30 T, Frequency 1000 Hz | 46.3 W/lb @Magnetic Field 1.30 T, Frequency 1000 Hz |
| 109 W/kg @Magnetic Field 1.00 T, Frequency 1500 Hz | 49.4 W/lb @Magnetic Field 1.00 T, Frequency 1500 Hz |
| 112 W/kg @Magnetic Field 1.00 T, Frequency 1500 Hz | 50.8 W/lb @Magnetic Field 1.00 T, Frequency 1500 Hz |
| 113 W/kg @Magnetic Field 0.200 T, Frequency 10000 Hz | 51.3 W/lb @Magnetic Field 0.200 T, Frequency 10000 Hz |
| 115 W/kg @Magnetic Field 0.200 T, Frequency 10000 Hz | 52.2 W/lb @Magnetic Field 0.200 T, Frequency 10000 Hz |
| 121 W/kg @Magnetic Field 0.700 T, Frequency 2500 Hz | 54.9 W/lb @Magnetic Field 0.700 T, Frequency 2500 Hz |
| 125 W/kg @Magnetic Field 0.700 T, Frequency 2500 Hz | 56.7 W/lb @Magnetic Field 0.700 T, Frequency 2500 Hz |
| 128 W/kg @Magnetic Field 0.400 T, Frequency 5000 Hz | 58.1 W/lb @Magnetic Field 0.400 T, Frequency 5000 Hz |
| 128 W/kg @Magnetic Field 0.400 T, Frequency 5000 Hz | 58.1 W/lb @Magnetic Field 0.400 T, Frequency 5000 Hz |
| 164 W/kg @Magnetic Field 1.20 T, Frequency 1500 Hz | 74.4 W/lb @Magnetic Field 1.20 T, Frequency 1500 Hz |
| 168 W/kg @Magnetic Field 1.20 T, Frequency 1500 Hz | 76.2 W/lb @Magnetic Field 1.20 T, Frequency 1500 Hz |
| 200 W/kg @Magnetic Field 1.30 T, Frequency 1500 Hz | 90.7 W/lb @Magnetic Field 1.30 T, Frequency 1500 Hz |
| 200 W/kg @Magnetic Field 1.30 T, Frequency 1500 Hz | 90.7 W/lb @Magnetic Field 1.30 T, Frequency 1500 Hz |
| 254 W/kg @Magnetic Field 1.00 T, Frequency 2500 Hz | 115 W/lb @Magnetic Field 1.00 T, Frequency 2500 Hz |
| 265 W/kg @Magnetic Field 1.00 T, Frequency 2500 Hz | 120 W/lb @Magnetic Field 1.00 T, Frequency 2500 Hz |
| 380 W/kg @Magnetic Field 0.700 T, Frequency 5000 Hz | 172 W/lb @Magnetic Field 0.700 T, Frequency 5000 Hz |
| 382 W/kg @Magnetic Field 0.700 T, Frequency 5000 Hz | 173 W/lb @Magnetic Field 0.700 T, Frequency 5000 Hz |
| 395 W/kg @Magnetic Field 0.400 T, Frequency 10000 Hz | 179 W/lb @Magnetic Field 0.400 T, Frequency 10000 Hz |
| 398 W/kg @Magnetic Field 0.400 T, Frequency 10000 Hz | 181 W/lb @Magnetic Field 0.400 T, Frequency 10000 Hz |
| 842 W/kg @Magnetic Field 1.00 T, Frequency 5000 Hz | 382 W/lb @Magnetic Field 1.00 T, Frequency 5000 Hz |
| 843 W/kg @Magnetic Field 1.00 T, Frequency 5000 Hz | 382 W/lb @Magnetic Field 1.00 T, Frequency 5000 Hz |
|
Component Elements Properties | Metric | English | Comments |
---|
Aluminum, Al | 0.70 % | 0.70 % |
Iron, Fe | 96.65 % | 96.65 % |
Silicon, Si | 2.65 % | 2.65 % |
|
Descriptive Properties |
---|
Magnetic Induction at 5000 A/m (T) | 1.65 |
Saturation Induction (T) | 1.99 |