Physical Properties | Original Value | Comments |
---|
Density | 7.65 g/cc |
Thickness | 200 - 240 microns |
| 230 microns |
|
Mechanical Properties | Original Value | Comments |
---|
Knoop Microhardness | 173 |
Hardness, Rockwell B | 83 |
Tensile Strength, Ultimate | 359 MPa |
Tensile Strength, Yield | 345 MPa |
Elongation at Break | 11 % |
Modulus of Elasticity | 113.8 GPa |
| 138 GPa |
| 203 GPa |
| 241 GPa |
| 276 GPa |
|
Electrical Properties | Original Value | Comments |
---|
Exciting Power (RMS) | 0.00260 RMS VA/lb @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00330 RMS VA/lb @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.00910 RMS VA/lb @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.0114 RMS VA/lb @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0190 RMS VA/lb @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0238 RMS VA/lb @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0315 RMS VA/lb @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0397 RMS VA/lb @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0465 RMS VA/lb @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0588 RMS VA/lb @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0637 RMS VA/lb @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.0807 RMS VA/lb @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.0834 RMS VA/lb @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1055 RMS VA/lb @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.1059 RMS VA/lb @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.1309 RMS VA/lb @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.1341 RMS VA/lb @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.1609 RMS VA/lb @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.1668 RMS VA/lb @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.1968 RMS VA/lb @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.2045 RMS VA/lb @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.2405 RMS VA/lb @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.2505 RMS VA/lb @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.2945 RMS VA/lb @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.305 RMS VA/lb @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.3614 RMS VA/lb @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.3723 RMS VA/lb @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.4455 RMS VA/lb @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.4545 RMS VA/lb @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.5568 RMS VA/lb @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.5582 RMS VA/lb @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.6927 RMS VA/lb @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.7545 RMS VA/lb @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.9273 RMS VA/lb @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.3045 RMS VA/lb @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.5818 RMS VA/lb @Magnetic Field 1.80 T, Frequency 60 Hz |
| 4.5136 RMS VA/lb @Magnetic Field 1.90 T, Frequency 50 Hz |
| 5.5409 RMS VA/lb @Magnetic Field 1.90 T, Frequency 60 Hz |
Electrical Resistivity | 0.0000500 ohm-cm |
|
Magnetic Properties | Original Value | Comments |
---|
Core Loss | 0.00289 W/kg @Magnetic Field 0.100 T, Frequency 50 Hz |
| 0.00385 W/kg @Magnetic Field 0.100 T, Frequency 60 Hz |
| 0.01082 W/kg @Magnetic Field 0.200 T, Frequency 50 Hz |
| 0.01451 W/kg @Magnetic Field 0.200 T, Frequency 60 Hz |
| 0.0236 W/kg @Magnetic Field 0.300 T, Frequency 50 Hz |
| 0.0317 W/kg @Magnetic Field 0.300 T, Frequency 60 Hz |
| 0.0413 W/kg @Magnetic Field 0.400 T, Frequency 50 Hz |
| 0.0554 W/kg @Magnetic Field 0.400 T, Frequency 60 Hz |
| 0.0635 W/kg @Magnetic Field 0.500 T, Frequency 50 Hz |
| 0.0852 W/kg @Magnetic Field 0.500 T, Frequency 60 Hz |
| 0.0903 W/kg @Magnetic Field 0.600 T, Frequency 50 Hz |
| 0.121 W/kg @Magnetic Field 0.600 T, Frequency 60 Hz |
| 0.1218 W/kg @Magnetic Field 0.700 T, Frequency 50 Hz |
| 0.1578 W/kg @Magnetic Field 0.800 T, Frequency 50 Hz |
| 0.1628 W/kg @Magnetic Field 0.700 T, Frequency 60 Hz |
| 0.1984 W/kg @Magnetic Field 0.900 T, Frequency 50 Hz |
| 0.211 W/kg @Magnetic Field 0.800 T, Frequency 60 Hz |
| 0.244 W/kg @Magnetic Field 1.00 T, Frequency 50 Hz |
| 0.265 W/kg @Magnetic Field 0.900 T, Frequency 60 Hz |
| 0.296 W/kg @Magnetic Field 1.10 T, Frequency 50 Hz |
| 0.325 W/kg @Magnetic Field 1.00 T, Frequency 60 Hz |
| 0.354 W/kg @Magnetic Field 1.20 T, Frequency 50 Hz |
| 0.394 W/kg @Magnetic Field 1.10 T, Frequency 60 Hz |
| 0.418 W/kg @Magnetic Field 1.30 T, Frequency 50 Hz |
| 0.470 W/kg @Magnetic Field 1.20 T, Frequency 60 Hz |
| 0.487 W/kg @Magnetic Field 1.40 T, Frequency 50 Hz |
| 0.555 W/kg @Magnetic Field 1.30 T, Frequency 60 Hz |
| 0.565 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.570 W/kg @Magnetic Field 1.50 T, Frequency 50 Hz |
| 0.648 W/kg @Magnetic Field 1.40 T, Frequency 60 Hz |
| 0.655 W/kg @Magnetic Field 1.60 T, Frequency 50 Hz |
| 0.750 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.750 W/kg @Magnetic Field 1.50 T, Frequency 60 Hz |
| 0.770 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.773 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.800 W/kg @Magnetic Field 1.70 T, Frequency 50 Hz |
| 0.867 W/kg @Magnetic Field 1.60 T, Frequency 60 Hz |
| 0.967 W/kg @Magnetic Field 1.80 T, Frequency 50 Hz |
| 1.01 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.017 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.06 W/kg @Magnetic Field 1.70 T, Frequency 60 Hz |
| 1.264 W/kg @Magnetic Field 1.80 T, Frequency 60 Hz |
| 1.365 W/kg @Magnetic Field 1.90 T, Frequency 50 Hz |
| 1.766 W/kg @Magnetic Field 1.90 T, Frequency 60 Hz |
|
Descriptive Properties |
---|
Approximate Equivalent International Grade | M080-23P5 |
Magnetostriction 10^8 | -18 |
| -20 |
| -20 |
| -21 |
Maximum Induction at 800 A/m (T) | 1.88 |
Minimum Lamination Factor (%) | 94.5 |
Typical Induction at 800 A/m (T) | 1.916 |
Typical Lamination Factor (%) | 96.6 |