MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Carlson 303 Austenitic Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Carlson 303 is an austenitic free-machining stainless steel. The standard 18-8 stainless steels are more difficult to turn, mill and drill which restricts their use when considerable machining is required. The additional sulfur present in 303 assists in breaking up turnings which reduces drag on the cutting tool. This permits greater machining speed and tends to produce smoother machined finishes which in turn lowers production costs.

This material is not as resistant to general corrosion as is 304. It tends to form a rust film more readily in moist atmospheres and is very susceptible to pitting or localized corrosion in solutions of chlorides, iodides, or bromides. Under relatively dry conditions or in mildly corrosive environments, 303 resists rust. It also has good resistance to oxidation up to 1700°F. 303 is not recommended for vessels containing gases or liquids under high pressure. It is available as hot rolled, annealed and pickled (HRAP) or hot rolled, annealed only (HRA) plate.

Applications

Carlson 303 is utilized wherever a combination of good corrosion resistance and considerable machining is required for a part. Applications include aircraft fittings, computer motor holder rings, bushings, fittings, pump and valve parts, screw machine products, shafts and other parts requiring extensive machining.

Information provided by Carlson

Key Words: UNS S30300
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.283 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 160
Tensile Strength at Break 35000 psi
Tensile Strength, Yield 90000 psi
@Strain 0.2 %
Elongation at Break 50 %
Reduction of Area 55 %
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 433 ohm-cir-mil/ft
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.4 µin/in-°F
@Temperature 20.0 °C
Mean
Specific Heat Capacity 0.120 BTU/lb-°F
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.15 %
Chromium, Cr 17 - 19 %
Iron, Fe 67.05 - 74.85 %
Manganese, Mn <= 2.0 %
Molybdenum, Mo <= 0.60 %
Nickel, Ni 8.0 - 10 %
Phosphorus, P <= 0.20 %
Silicon, Si <= 1.0 %
Sulfur, S >= 0.15 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
304 Stainless Steel
303 Stainless Steel, annealed
301 Stainless Steel
Aluminum 6061-T6; 6061-T651
AK Steel 316 Austenitic Stainless steel

NCARLSO00 / 15807

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.