MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Solvay VTM® 260 series Epoxy Resin
Categories: Polymer; Thermoset; Epoxy

Material Notes: Description: VTM 260 series resins are toughened, 65 to 120° (149 to 248°F) curing temperature epoxy resin matrices specifically developed for oven vacuum bag processing of large structures. These resins are particularly suited to the marine and industrial markets.

Features & Benefits:

  • Outstanding vacuum only processing capability on a wide range of reinforcements
  • Flexible curing capability
  • Up to 30 days out life 12°C (70°F)
  • 12 months storage at -18°C (0°F)
  • Service temperature up to 100°C (212°F)
  • Available in ZPREG selective impregnation formats
  • Suitable for component and tooling manufacture
  • Fully co-curable with the VTM260 range of adhesives surfacing films and syntactic plies
Product Variants:
VTM263: High viscosity, low flow variant-suitable for selective impregnation of fabrics or full impregnation of lightweight fabric reinforcements
VTM264: Intermediate viscosity and tack-suitable for full impregnation of light and medium weight unidirectional and fabric reinforcements
VTM266: Low viscosity-suitable for the full impregnation of heavyweight fabric reinforcements up to 2400g/m2
VTM267: Controlled tack for sided impregnation and film infusion
VTM267FRB and VTM264FRB: Flame-retarded resin systems are also available, see (PDS1180)

Note 1: Material: VTM264/CF302-42%; Cure cycle: 5 hours at 80°C (179°F), oven vacuum bag cure
Note 2: Material: VTM264/T700-35%; Cure cycle: 5 hours at 80°C (179°F), oven vacuum bag cure

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/cc1 hr at 120°C
Storage Temperature -18.0 °C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 5800 psi90°, Note 2; ASTM D3039
 102000 psi0°, Note 1; ASTM D3039
 108000 psi90°, Note 1; ASTM D3039
 374000 psi0°, Note 2; ASTM D3039
Tensile Modulus 9.10 GPa90°, Note 2; ASTM D3039
 60.0 GPa0°, Note 1; ASTM D3039
 60.5 GPa90°, Note 1; ASTM D3039
 131 GPa0°, Note 2; ASTM D3039
Compressive Strength 182 MPa90°, Note 2; ASTM D3410
 540 MPa0°, Note 1; ASTM D3410
 560 MPa90°, Note 1; ASTM D3410
 1235 MPa0°, Note 2; ASTM D3410
Compressive Modulus 53000 MPa90°, Note 1; ASTM D3410
 54000 MPa0°, Note 1; ASTM D3410
 188000 MPa0°, Note 2; ASTM D3410
Shear Modulus 3.90 GPaIn-plane, Note 1; ASTM D3518
 3.94 GPaIn-plane, Note 2; ASTM D3518
Shear Strength 10300 psi0° Interlaminar, Note 1; ASTM D2344
 12400 psiIn-plane, Note 2; ASTM D3518
 12900 psi0° Interlaminar, Note 2; ASTM D2344
 13800 psiIn-plane, Note 1; ASTM D3518
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 100 °C
Glass Transition Temp, Tg 80.0 °CDMA E' 16 hrs at 65°C
 95.0 °CDMA E' 5 hrs at 80°C
 115 °CDMA E' 2 hrs at 100°C
 120 °CDMA E' 1 hr at 120°C
 
Processing PropertiesOriginal ValueComments
Cure Time 1.00 hour
@Temperature 120 °C
 2.00 hour
@Temperature 100 °C
 5.00 hour
@Temperature 80.0 °C
Shelf Life 12.0 Month

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AlzChem DYHARD® Epoxy Fluid System for Filament Winding
Overview of materials for Epoxy Cure Resin
Overview of materials for Epoxy, Thermally Conductive
Solvay MTM® 79 Epoxy Matrix with 50% CF1420 Carbon Fiber Composite
Solvay Thornel® P-120 Carbon Fiber/Epoxy Advanced Composite System

PCYTED165 / 180467

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.