MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Zytel® (PA66) 70G20HSL BK039B PA66-GF20  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, 20% Glass Fiber Filled

Material Notes: 20% glass fiber reinforced, heat stabilized,  lubricated polyamide 66

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.28 g/ccDAM; ISO 1183
Melt Density 1.12 g/cc
Water Absorption 6.8 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
 1.5 %
@Thickness 2.00 mm,
Time 86400 sec
wall thickness 2mm; DAM; Sim. to ISO 62
Moisture Absorption 2.10 %
@Thickness 2.00 mm
DAM; Sim. to ISO 62
Viscosity Number 148 cm³/gDAM; ISO 307, 1157, 1628
Linear Mold Shrinkage, Flow 0.0040 cm/cmDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.012 cm/cmDAM; ISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 8550%RH; ISO 2039-2
 102DAM; ISO 2039-2
Hardness, Rockwell R 11550%RH; ISO 2039-2
 122DAM; ISO 2039-2
Tensile Strength at Break 100 MPa50%RH; ISO 527-1/-2
 150 MPaDAM; ISO 527-1/-2
Elongation at Break 2.7 %DAM; ISO 527-1/-2
 7.0 %50%RH; ISO 527-1/-2
Tensile Modulus 5000 MPa50%RH; ISO 527-1/-2
 7200 MPaDAM; ISO 527-1/-2
Poissons Ratio 0.35DAM
 0.3550%RH
Izod Impact, Notched (ISO) 6.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 180/1A
 7.00 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 180/1A
 7.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1A
 9.00 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 180/1A
Charpy Impact Unnotched 45.0 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eU
 50.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
 50.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
 75.0 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 6.00 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eA
 6.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 9.00 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 179/1eA
Tensile Creep Modulus, 1 hour 4700 MPa50%RH; ISO 899-1
Tensile Creep Modulus, 1000 hours 3100 MPa50%RH; ISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+9 ohm-cm50%RH; IEC 62631-3-1
Surface Resistance 1.00e+12 ohm50%RH; IEC 62631-3-2
Comparative Tracking Index 400 VDAM; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 35.0 µm/m-°CDAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 111 µm/m-°CDAM; ISO 11359-1/-2
Specific Heat Capacity 2.33 J/g-°CMelt
Thermal Conductivity 0.160 W/m-KMelt
 0.300 W/m-K
Melting Point 263 °C10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 250 °CDAM; ISO 75-1/-2
Glass Transition Temp, Tg 80.0 °C10°C/min; DAM; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 0.710 mm
DAM; IEC 60695-11-10
 HB
@Thickness 1.50 mm
DAM; IEC 60695-11-10
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
ISO 3795 (FMVSS 302)
 
Processing PropertiesOriginal ValueComments
Melt Temperature 285 - 305 °CInjection
 295 °COptimum, Injection
Mold Temperature 70.0 - 120 °CInjection
 100 °COptimum, Injection
Drying Temperature 80.0 °C
@Time 7200 - 14400 sec
Injection; Dehumidified Dryer
Moisture Content 0.20 %
Hold Pressure 50.0 - 100 MPaInjection
 
Descriptive Properties
AdditivesLubricants
 Release agent
Delivery formPellets
Drying Recommendedyes
Eff. thermal diffusivity7.20E-08 m²/s
FeaturesHeat stabilized or stable to heat
FMVSS ClassBISO 3795 (FMVSS 302)
Fogging, G-value (condensate)0.5 (mg)ISO 6452; DAM
Hold pressure time (s/mm)3Injection
ISO designationISO 16396-PA66,GF20,M1CGHR,S14-070
Max. screw tangential speed (m/s)0.2
Odor Class3.5VDA 270
Part Marking Code>PA66-GF20<ISO 11469
ProcessingInjection Molding
Regional AvailabilityEurope
 Near East/Africa
Resin IdentificationPA66-GF20ISO 1043
UL 94 recognitionyes
 yes

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDSX5319k / 254524

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.