MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
AK Steel 13-4 SR® Ferritic Stainless Steel
Categories: Metal; Ferrous Metal; Stainless Steel

Material Notes: AK Steel 13-4 SR Stainless Steel is a ductile weldable ferritic with 13% Cr and 3.75% Al. The high aluminum content results in a base alloy with high electrical resistivity. It is intended for use where electrical energy needs to be dissipated or heat is generated. Good oxidation resistance to 1800°F (982°C) permits applications at elevated temperatures. The alloy’s wet corrosion resistance is comparable to ferritic alloys Type 409 or Type 430.

Information provided by AK Steel.

Key Words: Classified in ASTM B603 Class IV and as UNS K91470
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 6.95 g/cc
@Temperature 1230 °C
 7.00 g/cc
@Temperature 1090 °C
 7.05 g/cc
@Temperature 954 °C
 7.105 g/cc
@Temperature 816 °C
 7.15 g/cc
@Temperature 677 °C
 7.195 g/cc
@Temperature 538 °C
 7.24 g/cc
@Temperature 399 °C
 7.285 g/cc
@Temperature 260 °C
 7.33 g/cc
@Temperature 121 °C
 7.36 g/cc
@Temperature -17.8 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 86
Tensile Strength, Ultimate 558 MPaLongitudinal Orientation, True Stress/True Strain
 586 MPaTransverse Orientation, True Stress/True Strain
Tensile Strength, Yield 421 MPa
@Strain 0.2 %
Longitudinal Orientation, True Stress/True Strain
 448 MPa
@Strain 0.2 %
Transverse Orientation, True Stress/True Strain
Elongation at Break 22 %Transverse Orientation, In 2", True Stress/True Strain
 28 %Longitudinal Orientation, In 2", True Stress/True Strain
Rupture Strength 3.70 MPa
@Temperature 871 °C,
Time 3.60e+6 sec
Stress Rupture Strength
 6.30 MPa
@Temperature 871 °C,
Time 360000 sec
Stress Rupture Strength
 8.30 MPa
@Temperature 760 °C,
Time 3.60e+6 sec
Stress Rupture Strength
 15.9 MPa
@Temperature 760 °C,
Time 360000 sec
Stress Rupture Strength
 31.0 MPa
@Temperature 649 °C,
Time 3.60e+6 sec
Stress Rupture Strength
 46.5 MPa
@Temperature 649 °C,
Time 360000 sec
Stress Rupture Strength
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.79 µin/in-°F
@Temperature 100 °C
 10.6 µin/in-°F
@Temperature 200 °C
 11.2 µin/in-°F
@Temperature 300 °C
 11.65 µin/in-°F
@Temperature 400 °C
 12.05 µin/in-°F
@Temperature 500 °C
 12.38 µin/in-°F
@Temperature 600.0 °C
 12.6 µin/in-°F
@Temperature 700.0 °C
 12.99 µin/in-°F
@Temperature 800.0 °C
 13.36 µin/in-°F
@Temperature 900.0 °C
 13.66 µin/in-°F
@Temperature 1000 °C
Thermal Conductivity 13.7 W/m-K
@Temperature 22.8 °C
 14.2 W/m-K
@Temperature 50.0 °C
 15.0 W/m-K
@Temperature 100 °C
 16.6 W/m-K
@Temperature 200 °C
 18.2 W/m-K
@Temperature 300 °C
 19.8 W/m-K
@Temperature 400 °C
 20.5 W/m-K
@Temperature 700.0 °C
 22.8 W/m-K
@Temperature 500 °C
 24.0 W/m-K
@Temperature 800.0 °C
 24.8 W/m-K
@Temperature 900.0 °C
 25.1 W/m-K
@Temperature 600.0 °C
 26.2 W/m-K
@Temperature 1000 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 3.75 %
Carbon, C 0.025 %
Chromium, Cr 13 %
Iron, Fe 82 - 82.375 %Balance
Manganese, Mn 0.30 %
Nickel, Ni 0.25 %
Phosphorus, P <= 0.045 %
Sulfur, S <= 0.030 %
Titanium, Ti 0.30 %
 
Descriptive Properties
100 Hour Still Air Oxidation Resistance, Weight Gain (mg/cm2)0.191600°F
 0.411800°F
 1.022000°F
 3.232200°F
Cyclic Oxidation Resistance 1550°-1600°F, Weight Change (mg/cm2)0.12100 cycles
 0.13200 cycles
 0.17300 cycles
 0.18400 cycles
 0.18500 cycles
n Value (10% -Ult)0.147Transverse Orientation,True Stress/True Strain
 0.167Longitudinal Orientation, True Stress/True Strain

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ATI Allegheny Ludlum ALFA-I™ Stainless Steel Type 406
ATI Allegheny Ludlum Stainless Steel Ohmaloy® 40 Resistance Alloy
406 Stainless Steel
Aluminum 6061-T6; 6061-T651
ATI Allegheny Ludlum ALFA-II™ Stainless Steel Type 406

NAKS091a / 140765

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.