MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
3M Dyneon™ 131T High Temperature Perfluoroelastomer
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: 3M™ Dyneon™ 131TZ is a technically advanced high temperature perfluoroelastomer (HT PFE). It is designed to meet the challenges of higher temperature applications. It is classified as FFKM per ASTM D1418. Its fully fluorinated back bone structure provides a very broad chemical and thermal stability.

    Features and Benefits:
  • Ideal for dry side (thermal processes) semiconductor applications including plasma, and high temperature CPI and aerospace applications
  • High temperature FFKM
  • Low metal ion content with low extractables
  • Upper use temperature of 315°C
  • Excellent compression set resistance
  • Can be compounded to pass AMS 7257C

Information provided by the Dyneon division of 3M.

Key Words: Formerly 131TZ
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.00 g/cc
Mooney Viscosity 80
@Temperature 121 °C
ML 1+ 10
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 77Press Cure 10 Minutes @ 188°C, Post Cure 16 Hours @ 250°C
Tensile Strength at Break 15.9 MPaPress Cure 10 Minutes @ 188°C, Post Cure 16 Hours @ 250°C
Elongation at Break 165 %Press Cure 10 Minutes @ 188°C, Post Cure 16 Hours @ 250°C
100% Modulus 0.00910 GPa
@Strain 100 %
Press Cure 10 Minutes @ 188°C, Post Cure 16 Hours @ 250°C
Compression Set 20 %
@Treatment Temp. 232 °C,
Time 252000 sec
Method B, -214 O-rings, Aged 70 Hours, 25% Deformation; ASTM D395
 25 %
@Treatment Temp. 232 °C,
Time 605000 sec
Method B, -214 O-rings, Aged 168 Hours, 25% Deformation; ASTM D395
 43 %
@Treatment Temp. 300 °C,
Time 252000 sec
Method B, -214 O-rings, Aged 70 Hours, 18% Deformation; ASTM D395
 52 %
@Treatment Temp. 300 °C,
Time 252000 sec
Method B, -214 O-rings, Aged 70 Hours, 18% Deformation; ASTM D395
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 315 °C
Brittleness Temperature -35.0 °C
Transformation Temperature -2.00 °CTR10
 
Descriptive Properties
ColorWhite
FormCrumb
MH, Maximum Toque17.8 Inch-lb100 cpm, 0.5° Arc, 12 Minutes @ 188°C, ASTM D5289
ML, Minimum Torque1.2 Inch-lb100 cpm, 0.5° Arc, 12 Minutes @ 188°C, ASTM D5289
t2, Time to 2 Inch-lb Rise from Minimum2.4 Minutes100 cpm, 0.5° Arc, 12 Minutes @ 188°C, ASTM D5289
t'50, Time to 50% Cure3.6 Minutes100 cpm, 0.5° Arc, 12 Minutes @ 188°C, ASTM D5289
t'90, Time to 90% Cure7.0 Minutes100 cpm, 0.5° Arc, 12 Minutes @ 188°C, ASTM D5289

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
3M Dyneon™ FC 2110Q Fluoroelastomer
3M Dyneon™ PFE 80Z Peroxide Cure Perfluoroelastomer
DuPont Mobility and Materials Kalrez® AeroSeal™ 7797 Fluoroelastomer
Freudenberg Simriz® 481 Low Temperature FFKT Perfluoroelastomer Compound
3M Dyneon™ TFE 90 Peroxide Cure Perfluoroelastomer

PDYL9966 / 129984

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.