MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Copper Alloy, UNS C64780, H04 Temper, Flat Products
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: Hard

Fabrication Properties: Excellent Suitability – Soldering; Good Suitability – Brazing, Gas Shielded Arc Welding, Spot Weld, Capacity for Being Cold Worked, Capacity for Being Hot Formed

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.321 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 185
@Load 0.500 kg
Tensile Strength 86.0 ksi
Tensile Strength, Yield 78.0 ksi0.2% Offset
Elongation at Break 10 %
Tensile Modulus 11600 ksi
Modulus of Rigidity 4400 ksi
Poissons Ratio 0.32Calculated
Fatigue Strength 35000 psi
@# of Cycles 1.00e+8
Machinability 20 %
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000360 ohm-cm48% IACS
 
Thermal PropertiesOriginal ValueComments
Specific Heat Capacity 0.0950 BTU/lb-°F
Thermal Conductivity 116.2 BTU-in/hr-ft²-°F
Melting Point 1954 - 1989 °F
Solidus 1954 °F
Liquidus 1989 °F
Annealing Point >= 842 °F
 
Processing PropertiesOriginal ValueComments
Processing Temperature >= 482 °FStress Relief
Hot-Working Temperature 1382 - 1832 °F
 
Component Elements PropertiesOriginal ValueComments
Chromium, Cr <= 0.010 %
Copper, Cu >= 90 %
Lead, Pb <= 0.020 %
Magnesium, Mg <= 0.010 %
Manganese, Mn 0.010 - 1.0 %
Nickel, Ni 1.0 - 3.5 %
Silicon, Si 0.20 - 0.90 %
Tin, Sn 0.10 - 2.0 %
Titanium, Ti <= 0.010 %
Zinc, Zn 0.20 - 2.5 %
Zirconium, Zr <= 0.010 %
 
Descriptive Properties
Proportional Limit70 ksi
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

MC64780x4 / 292250

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.