MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Thermal Ceramics FireMaster Firecrete 85
Categories: Ceramic; Ceramic Matrix Composite

Material Notes: Firecrete 85 is used on fire training facility wall and ceiling constructions. It is a high-strength insulating refractory castable which offers superior thermal shock resistance and spall resistance when exposed to repeated hose stream conditions at high temperatures. This performance is achieved by the incorporation of RFT (Rapid Fire Technology) and stainless steel fibers.

Features:

  • Superior thermal shock resistance, which provides spall resistance
  • Lightweight
  • Low thermal conductivity
  • High strength
  • Abrasion resistance
  • Information provided by Thermal Ceramics

    Data has not been recently verified. Please contact manufacturer for current information.

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesOriginal ValueComments
    Density 1.346 g/cc
     
    Mechanical PropertiesOriginal ValueComments
    Modulus of Rupture 0.400 - 0.600 ksiDried 18-24 hours at 220°F
     0.275 - 0.400 ksi
    @Treatment Temp. 816 °C,
    Time 18000 sec
     0.900 - 1.20 ksi
    @Treatment Temp. 1430 °C,
    Time 18000 sec
    Compressive Strength 6.86 - 11.1 MPaFired 5 hours at 1500°F cast
     11.8 - 16.6 MPaDried for 18-24 hours at 220°F
     18.6 - 23.4 MPaFired 5 hours at 2600°F cast
     
    Thermal PropertiesOriginal ValueComments
    Thermal Conductivity 2.30 BTU-in/hr-ft²-°F
    @Temperature 260 °C
    ASTM C417-86
     2.40 BTU-in/hr-ft²-°F
    @Temperature 538 °C
    ASTM C417-86
     2.60 BTU-in/hr-ft²-°F
    @Temperature 1090 °C
    ASTM C417-86
    Melting Point 2700 °F
    Maximum Service Temperature, Air 2500 °F
    Shrinkage 0.10 - 0.40 %
    @Temperature 816 °C,
    Time 18000 sec
     0.00 - 0.20 %
    @Treatment Temp. 104 °C
    Dried 18-24 hours
     
    Component Elements PropertiesOriginal ValueComments
    Al2O3 42 %
    Alkalis 0.70 %
    CaO 16.2 %
    Fe2O3 2.6 %
    SiO2 37 %
    TiO2 1.5 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    Silicon Carbide, Reaction-Bonded, SiSiC
    COI Ceramics Nextel™ AS-N312 Oxide Ceramic Matrix Composite, Aluminosilicate
    COI Ceramics Sylramic™ S300 Silicon Carbide Ceramic Matrix Composite, SiC
    Morgan Advanced Ceramics Vitox® AMC Alumina Matrix Composite Technical Ceramic
    UBE Tyrannohex® Heat Resistant Composite

    CTHERM113 / 2433

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.