MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPV 3450N Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 3450N is a general purpose thermoplastic vulcanizate used in consumer and industrial applications. Sarlink TPV 3450N is a low hardness, low density, RoHS compliant grade suitable for injection molding, blow molding, extrusion, and pipe extrusion.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; General Purpose; Good Adhesion; High Heat Resistant; Low Density; Low Hardness; Low Specific Gravity

Uses: Fittings; General Purpose; Piping; Potable Water Applications

RoHS Compliance: RoHS Compliant

Agency Ratings: NSF STD-61

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding; Pipe Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.940 g/ccASTM D792
Viscosity 270 cP
@Shear Rate 206 1/s,
Temperature 200 °C
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 54
@Time 5.00 sec
Extruded; ISO 868
 57
@Time 5.00 sec
Injection Molded; ISO 868
Tensile Strength at Break 479 psiFlow; ISO 37
 682 psiAcross Flow; ISO 37
Tensile Strength, Yield 479 psiFlow; ASTM D412
 682 psiAcross Flow; ASTM D412
Tensile Stress at Strain 261 psi
@Strain 100 %
Across Flow; ISO 37
 319 psi
@Strain 100 %
Flow; ISO 37
 274 psi
@Strain 100 %,
Treatment Temp. 150 °C
Across Flow, Change in Air at 168 hr; ISO 188
 279 psi
@Strain 100 %,
Treatment Temp. 135 °C
Across Flow, Change in Air at 1000 hr; ISO 188
Elongation at Break 320 %Flow; ISO 37
 580 %Across Flow; ISO 37
 539 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
Across Flow, Change in Air; ISO 188
 626 %
@Treatment Temp. 150 °C,
Time 605000 sec
Across Flow, Change in Air; ISO 188
Tear Strength 140 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set 20 %
@Temperature 22.8 °C,
Time 79200 sec
ISO 815
 37 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 41 %
@Temperature 125 °C,
Time 252000 sec
ISO 815
 
Processing PropertiesOriginal ValueComments
Processing Temperature 360 - 430 °FInjection
Rear Barrel Temperature 350 - 420 °FInjection
Middle Barrel Temperature 350 - 420 °FInjection
Front Barrel Temperature 350 - 420 °FInjection
Nozzle Temperature 370 - 430 °FInjection
Zone 1 360 - 400 °FExtrusion
Zone 2 360 - 400 °FExtrusion
Zone 3 370 - 410 °FExtrusion
Zone 4 370 - 410 °FExtrusion
Die Temperature 380 - 420 °FExtrusion
Melt Temperature 380 - 420 °FExtrusion
Mold Temperature 50.0 - 150 °FInjection
Drying Temperature 180 °F
Dry Time 3.00 hour
Screw Speed 100 - 200 rpmInjection
 
Descriptive Properties
AppearanceOpaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ1147 / 237638

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.