MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
ATI Allegheny Ludlum AL 13-8™ H 1050 Precipitation Hardening Alloy, Heat Treated at 1150°F
Categories: Metal; Ferrous Metal; Martensitic; Stainless Steel; Precipitation Hardening Stainless; T S10000 Series Stainless Steel

Material Notes:

Characteristics: excellent strength, high hardness, superior toughness, good corrosion resistance, good transverse toughness properties, strength and ductility can be tailored by varying the aging temperature.

Applications:large air frame structures, injection molding equipment.

Information provided by Allegheny Ludlum

Heat treated at 1150°F for 4 hrs

Key Words: UNS S13800, ASTM XM-13
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.76 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 33
Tensile Strength, Ultimate 931 MPa
Tensile Strength, Yield 621 MPa
@Strain 0.2 %
Elongation at Break 14 %in 2"
Reduction of Area 50 %Short-Transverse
 50 %Longitudinal
 50 %Transverse
Creep Strength 827 MPa
@Temperature 260 °C,
Time 36000 sec
Rupture Strength 930 MPa
@Temperature 260 °C,
Time 36000 sec
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.6 µm/m-°C
@Temperature 20.0 - 100 °C
Melting Point 1405 - 1470 °C
Solidus 1405 °C
Liquidus 1470 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.90 - 1.35 %
Carbon, C <= 0.050 %
Chromium, Cr 12.25 - 13.25 %
Iron, Fe >= 74.032 %As Remainder
Manganese, Mn <= 0.20 %
Molybdenum, Mo 2.0 - 2.5 %
Nickel, Ni 7.5 - 8.5 %
Phosphorus, P <= 0.010 %
Silicon, Si <= 0.10 %
Sulfur, S <= 0.0080 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI Type S15500 (15Cr-5Ni) Precipitation Hardening Stainless Steel transverse direction, condition H900
Overview of materials for Precipitation Hardening Stainless
17-7 PH Stainless Steel, CH900, plate, sheet, and strip
AISI Type S13800 Stainless Steel (PH 13-8 Mo) longitudinal properties, condition RH950
Nickel, Ni

NL1015 / 17783

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.