MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Lead, Pb
Categories: Metal; Nonferrous Metal; Lead Alloy; Pure Element

Material Notes: Lead is a soft, dense, ductile metal. Pure (utility) lead is used in lead-acid batteries (automobile batteries and related), ammunition and armor, counterweights, ballast, inertial components, sound insulation, and radiation shielding. Lead is a toxic element and precautions are needed to minimize human exposure.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 10.22 g/cc
@Temperature 800 °C
liquid
 10.37 g/cc
@Temperature 600 °C
liquid
 10.6 g/cc
@Temperature 400 °C
liquid
 10.7 g/cc
@Temperature 325 °C
liquid
 11.0 g/cc
@Temperature 300 °C
 11.15 g/cc
@Temperature 200 °C
 11.35 g/cc
@Temperature 25.0 °C
Viscosity 56500 cP
@Temperature 390 °C
Vapor Pressure 0.001013 bar
@Temperature 957 °C
 0.01013 bar
@Temperature 1140 °C
 0.1013 bar
@Temperature 1389 °C
 1.013 bar
@Temperature 1750 °C
Surface Tension 439 dynes/cm
@Temperature 390 °C
 
Chemical PropertiesOriginal ValueComments
Atomic Mass 207.21995
Atomic Number 82
Thermal Neutron Cross Section 0.17 barns/atom
X-ray Absorption Edge 0.14077 ÅK
 0.78153 ÅLI
 0.81552 ÅLII
 0.95112 ÅLIII
Electrode Potential -0.126 V
Electronegativity 1.8Pauling
Ionic Radius 0.840 ÅCrystal Ionic Radius for Valence +4
 1.20 ÅCrystal Ionic Radius for Valence +2
Electrochemical Equivalent 3.858 g/A/h
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 4.2Cast
Hardness, Vickers 5.0
Tensile Strength, Ultimate 18.0 MPa
Modulus of Elasticity 14.0 GPa
Poissons Ratio 0.42
Shear Modulus 4.90 GPacalculated
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000020643 ohm-cm
@Temperature 20.0 °C
 0.000027021 ohm-cm
@Temperature 100 °C
 0.000036378 ohm-cm
@Temperature 200 °C
 0.000047938 ohm-cm
@Temperature 300 °C
solid
 0.000097867 ohm-cm
@Temperature 340 °C
liquid
 0.000101 ohm-cm
@Temperature 400 °C
liquid
Magnetic Susceptibility -1.20e-7cgs/g
Critical Magnetic Field Strength, Oersted 802 - 804
Critical Superconducting Temperature 7.19 - 7.202 K3.55 K at 16.0 GPa pressure for Pb II
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 24.1 J/g
Heat of Vaporization 850 J/g
 866.3 J/gAt Boiling Point
CTE, linear 29.1 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.1004 J/g-°CGas
 0.1287 J/g-°C
@Temperature 25.0 °C
 0.132 J/g-°C
@Temperature 127 °C
 0.1368 J/g-°C
@Temperature 227 °C
 0.139 J/g-°C
@Temperature 827 °C
liquid
 0.1404 J/g-°C
@Temperature 727 °C
liquid
 0.1421 J/g-°C
@Temperature 327.4 °C
solid
 0.1433 J/g-°C
@Temperature 627 °C
liquid
 0.1449 J/g-°C
@Temperature 527 °C
liquid
 0.1465 J/g-°C
@Temperature 427 °C
liquid
 0.1479 J/g-°C
@Temperature 327.4 °C
liquid
Thermal Conductivity 33.0 W/m-K
Melting Point 327.5 °C
Boiling Point 1749 °C
Heat of Formation 0.000 kJ/molCrystal
 195.2 kJ/molGas
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.050
@Temperature 200 °C
Oxidized; total spectrum
 0.63
@Temperature 200 °C
Unoxidized total spectrum
Reflection Coefficient, Visible (0-1) 0.62589 nm
 
Component Elements PropertiesOriginal ValueComments
Lead, Pb 100 %
 
Descriptive Properties
CAS Number7439-92-1
SolubilitySoluble in concentrated Acid

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Copper, Cu; Annealed
Tungsten, W
Titanium, Ti
Gold, Au
Silver, Ag

AMEPb00 / 80

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.