MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Desmopan® 1085A TPU
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Injection molding grade; hydrolysis-stabilized; high mechanical strength; very short cycle times; Application; Injection molded engineering parts; Screenpacks

Mechanical property data for samples at 50% RH.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.208 g/ccISO 1183-1
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 85ISO 868
Tensile Strength, Ultimate 5220 psi200 mm/min; DIN 53504
Elongation at Break 716 %200 mm/min; DIN 53504
Tensile Modulus 23.0 MPa
@Temperature 60.0 °C
storage; ISO 6721-1,-4
 35.0 MPa
@Temperature 20.0 °C
storage; ISO 6721-1,-4
 210 MPa
@Temperature -20.0 °C
storage; ISO 6721-1,-4
100% Modulus 0.00520 GPa
@Strain 100 %
200 mm/min; DIN 53504
200% Modulus 0.00910 GPa
@Strain 200 %
200 mm/min; DIN 53504
Rebound 41 %Resilience; ISO 4662
Tear Strength 74.0 kN/m500 mm/min; ISO 34-1
Abrasion 11mm3; ISO 4649 method A
Compression Set 19 %
@Temperature 23.0 °C,
Time 259000 sec
ISO 815
 26 %
@Temperature 70.0 °C,
Time 86400 sec
DIN ISO 815-1, Method C
 34 %
@Temperature 70.0 °C,
Time 86400 sec
ISO 815
 
Processing PropertiesOriginal ValueComments
Melt Temperature 190 - 230 °C
Mold Temperature 20.0 - 40.0 °C
Drying Temperature 90.0 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
AISI 3310 Carburizing Bearing Steel
Covestro Desmopan® 1080AU TPU
Covestro Desmopan® 1092A TPU
AISI 12L15 Steel, cold drawn, 19-38 mm round
AISI 1215 Steel, cold drawn, 19-38 mm round

PCOVEST0689 / 202472

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.