MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

ATI Allegheny Ludlum AL-6XN PLUS™ Superaustenitic Stainless Steel
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel

Material Notes: Enhanced version of AL-6NX™, containing a greater concentration of the alloying elements which promote corrosion resistance.

Information provided by Allegheny Ludlum

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.020 %0.020 %
Chromium, Cr 21.8 %21.8 %
Copper, Cu 0.20 %0.20 %
Iron, Fe >= 45.069 %>= 45.069 %As Remainder
Manganese, Mn 0.30 %0.30 %
Molybdenum, Mo 6.7 %6.7 %
Nickel, Ni 25.3 %25.3 %
Nitrogen, N 0.24 %0.24 %
Phosphorus, P 0.020 %0.020 %
Silicon, Si 0.35 %0.35 %
Sulfur, S <= 0.0010 %<= 0.0010 %
 
Descriptive Properties
Critical Crevice Corrosion Temperature, °C45 (ASTM G48, Practice D)Acified Ferric Chloride solution, Pickled Mill surface
 55 (ASTM G48, Practice B)Acified Ferric Chloride solution, Pickled Mill surface
Critical Pitting Temperature, °C90 (ASTM G48, Practice C)Acified Ferric Chloride solution, Pickled Mill surface
Electrochemical Critical Pitting Temperature, °C90 (ASTM G150)1M NaCl solution, Ground Surface
Pitting Resistance Equivalent (PREN)50.0 Minimum

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allvac® AL 6XN® UNS N08367 Specialty Steel
Crucible Steel SUE52 Martensitic Steel
MetalTek MTEK 6XN Cast UNS J94651 Super Austenitic Stainless Steel
ATI Allegheny Ludlum AL 29-4® Superferritic Stainless Steel, UNS S44700
ATI Allegheny Ludlum 316Ti Austenitic Stainless Steel

NL1024 / 17792

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.