MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

(Viewing data as-entered. Click here to return)
Special Metals NIMONIC® alloy 91 Ni-Cr-Co Alloy
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Nickel Alloy

Material Notes: NIMONIC® alloy 91 is a wrought nickel-chromium-cobalt based alloy strengthened by additions of aluminum and titanium.

This alloy is a modification of NIMONIC alloy 90, but has an increased chromium content to improve corrosion resistance in salt and sulfur contaminated environments. The alloy is suitable for long service up to about 900°C. It combines good strength and ductility with stability of microstructure and excellent resistance to hot corrosion.

NIMONIC alloy 91 is intended for high-temperature stressed parts such as blades in gas turbines, burning impure fuels or operating in marine environments.

Information Provided by Special Metals Corporation

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.08 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 96.0 MPa
@Temperature 1000 °C
 365 MPa
@Temperature 900 °C
 644 MPa
@Temperature 800 °C
 947 MPa
@Temperature 700 °C
 993 MPa
@Temperature 600 °C
 1001 MPa
@Temperature 400 °C
 1126 MPa
@Temperature 200 °C
 1180 MPa
@Temperature 20.0 °C
Tensile Strength, Yield 59.0 MPa
@Strain 0.1 %,
Temperature 1000 °C
 61.0 MPa
@Strain 0.2 %,
Temperature 1000 °C
 293 MPa
@Strain 0.1 %,
Temperature 900 °C
 315 MPa
@Strain 0.2 %,
Temperature 900 °C
 530 MPa
@Strain 0.1 %,
Temperature 600 °C
 533 MPa
@Strain 0.1 %,
Temperature 400 °C
 535 MPa
@Strain 0.1 %,
Temperature 800 °C
 544 MPa
@Strain 0.2 %,
Temperature 400 °C
 547 MPa
@Strain 0.2 %,
Temperature 600 °C
 556 MPa
@Strain 0.2 %,
Temperature 800 °C
 561 MPa
@Strain 0.1 %,
Temperature 700 °C
 581 MPa
@Strain 0.2 %,
Temperature 700 °C
 599 MPa
@Strain 0.1 %,
Temperature 200 °C
 610 MPa
@Strain 0.2 %,
Temperature 200 °C
 657 MPa
@Strain 0.1 %,
Temperature 20.0 °C
 663 MPa
@Strain 0.2 %,
Temperature 20.0 °C
Elongation at Break 21.6 %
@Temperature 600 °C
 22.4 %
@Temperature 900 °C
 25.6 %
@Temperature 800 °C
 28 %
@Temperature 700 °C
 28 %
@Temperature 400 °C
 29.6 %
@Temperature 200 °C
 31.2 %
@Temperature 20.0 °C
 137.8 %
@Temperature 1000 °C
Reduction of Area 23.5 %
@Temperature 600 °C
 24.2 %
@Temperature 900 °C
 24.9 %
@Temperature 800 °C
 26.6 %
@Temperature 400 °C
 27.9 %
@Temperature 700 °C
 29.3 %
@Temperature 20.0 °C
 31.5 %
@Temperature 200 °C
 98 %
@Temperature 1000 °C
Rupture Strength 139 MPa
@Temperature 870 °C,
Time 533000 sec
cold-rolled; 12.8% elongation
 250 MPa
@Temperature 815 °C,
Time 338000 sec
forged; 8.4% elong
 386 MPa
@Temperature 750 °C,
Time 266000 sec
forged; 4.4% elong
Modulus of Elasticity 132 GPa
@Temperature 900 °C
 149 GPa
@Temperature 700 °C
 163 GPa
@Temperature 500 °C
 195 GPa
@Temperature 300 °C
 204 GPa
@Temperature 100 °C
 222 GPa
@Temperature 20.0 °C
Impact Test 16.3 J
@Temperature 750 °C,
Time 7.27e+6 sec
Soaking Time: 2020 hours at 750°C
 32.5 - 38.0 J
@Treatment Temp. 850 °C,
Time 3.60e+6 sec
Soaking Time: 1000 hours at 850°C
 
Thermal PropertiesOriginal ValueComments
Specific Heat Capacity 0.447 J/g-°C
@Temperature 20.0 °C
 0.468 J/g-°C
@Temperature 100 °C
 0.521 J/g-°C
@Temperature 300 °C
 0.574 J/g-°C
@Temperature 500 °C
 0.627 J/g-°C
@Temperature 700 °C
 0.680 J/g-°C
@Temperature 900 °C
Melting Point >= 1300 °C
 1350 °C
Solidus 1300 °C
Liquidus 1350 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.90 - 1.5 %
Boron, B 0.0020 - 0.010 %
Carbon, C <= 0.10 %
Chromium, Cr 27 - 30 %
Cobalt, Co 19 - 21 %
Copper, Cu <= 0.50 %
Iron, Fe <= 1.0 %
Manganese, Mn <= 1.0 %
Nickel, Ni 39.99 - 50.798 %Balance
Niobium, Nb (Columbium, Cb) 0.40 - 1.1 %
Silicon, Si <= 1.0 %
Titanium, Ti 1.9 - 2.7 %
Zirconium, Zr <= 0.10 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Special Metals INCONEL® Alloy 718
Special Metals NIMONIC® Alloy 90
Special Metals NIMONIC® Alloy 80A
Haynes 282® Nickel Alloy Sheet, Solution Annealed and Age-hardened
Special Metals INCONEL® Alloy X-750

NINDA15 / 98906

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.