MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Hexcel® HiFlow® 1078-1 Bi-component Epoxy System
Categories: Polymer; Thermoset; Epoxy

Material Notes: Description: HiFlow® 1078-1 is an aerospace bi-component resin system with liquid Part A & Part B specially developed for Liquid Composite Molding technologies, such as LRI and RTM. Delivered as two component system, HiFlow® 1078-1 provides several benefits over a mono-component resin: air shipment is allowed, storage at 23± 5°C for 12 months and larger packages are possible. HiFlow® 1078-1 Part A:B mixing ratio by weight is 100 : 63. HiFlow® 1078-1 presents services temperatures from -60°C up to 120°C with greater toughness, Tg stability and cycle processing flexibility making it ideal for primary and secondary aerospace structures. Long injection windows due to HiFlow® 1078-1 low viscosity are also easily reached, facilitating large parts manufacturing. HiFlow® 1078-1 resin can be used in combination with HexForce®, HiTape® & HiMax® reinforcements. HiFlow® 1078-1 is fully compatible with Hexcel binders and veils. They provide easy preforming properties and reinforcement dimensional stability.

Advantages

  • High glass transition temperatures: dry1: Tg> 200°C; wet2: Tg> 170°C
  • Low moisture absorption: 1,0 – 2,0%
  • < 100mPa.s at process temperatures
  • Toughened system
  • Liquid Part A & Part B at room temperature
  • Longer shelf life (12 months at RT), as bicomponent system

Information provided by Hexcel Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.12 g/cc
Moisture Absorption 1.00 - 2.00 %
Viscosity 9.00 cP
@Temperature 180 °C
3°C/min
 10.0 cP
@Temperature 175 °C
2°C/min
 12.0 cP
@Temperature 150 °C
1°C/min
 20.0 cP
@Temperature 140 °C
0.5°C/min
 10000 cP
@Temperature 48.0 °C
0.5°C/min
 10000 cP
@Temperature 152 °C
0.5°C/min
 10000 cP
@Temperature 48.0 °C
1°C/min
 10000 cP
@Temperature 175 °C
1°C/min
 10000 cP
@Temperature 48.0 °C
2°C/min
 10000 cP
@Temperature 197 °C
2°C/min
 10000 cP
@Temperature 48.0 °C
3°C/min
 10000 cP
@Temperature 210 °C
3°C/min
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 30.0 MPa
@Temperature 120 °C
Wet; ASTM D638
 55.0 MPa
@Temperature 120 °C
Dry; ASTM D638
 70.0 MPa
@Temperature 23.0 °C
Wet; ASTM D638
 90.0 MPa
@Temperature 23.0 °C
Dry; ASTM D638
Tensile Modulus 1.70 GPa
@Temperature 120 °C
Wet; ASTM D638
 2.30 GPa
@Temperature 120 °C
Dry; ASTM D638
 2.80 GPa
@Temperature 23.0 °C
Wet; ASTM D638
 3.00 GPa
@Temperature 23.0 °C
Dry; ASTM D638
Compressive Yield Strength 60.0 MPa
@Temperature 120 °C
Wet; ASTM D695
 80.0 MPa
@Temperature 120 °C
Dry; ASTM D695
 120 MPa
@Temperature 23.0 °C
Wet; ASTM D695
 130 MPa
@Temperature 23.0 °C
Dry; ASTM D695
Compressive Strength 240 MPaafter 30J impact; ASTM D7136/ D7137
 250 MPaafter 15J impact; ASTM D7136/ D7137
 435 MPa
@Temperature 115 - 125 °C
0°, Ultimate, Wet; EN2850A1
 490 MPa
@Temperature 115 - 125 °C
0°, Ultimate, Dry; EN2850A1
 620 MPa
@Temperature 18.0 - 28.0 °C
0°, Ultimate, Dry; EN2850A1
 625 MPa
@Temperature 18.0 - 28.0 °C
0°, Ultimate, Wet; EN2850A1
Compressive Modulus 2400 MPa
@Temperature 120 °C
Dry; ASTM D695
 2400 MPa
@Temperature 120 °C
Wet; ASTM D695
 2900 MPa
@Temperature 23.0 °C
Wet; ASTM D695
 3100 MPa
@Temperature 23.0 °C
Dry; ASTM D695
Fracture Toughness 0.637 ksi-in½
Shear Modulus 3.00 GPa
@Temperature 115 - 125 °C
In plane, Wet; EN6031
 3.40 GPa
@Temperature 115 - 125 °C
In plane, Dry; EN6031
 3.60 GPa
@Temperature 85.0 - 95.0 °C
In plane, Wet; EN6031
 3.70 GPa
@Temperature 65.0 - 75.0 °C
In plane, Wet; EN6031
 3.90 GPa
@Temperature 18.0 - 28.0 °C
In plane, Wet; EN6031
 4.10 GPa
@Temperature 18.0 - 28.0 °C
In plane, Dry; EN6031
Shear Strength 65.0 MPa
@Temperature 115 - 125 °C
Ultimate, In plane, Wet; EN6031
 80.0 MPa
@Temperature 115 - 125 °C
Ultimate, In plane, Dry; EN6031
 80.0 MPa
@Temperature 85.0 - 95.0 °C
Ultimate, In plane, Wet; EN6031
 85.0 MPa
@Temperature 65.0 - 75.0 °C
Ultimate, In plane, Wet; EN6031
 105 MPa
@Temperature 18.0 - 28.0 °C
Ultimate, In plane, Wet; EN6031
 110 MPa
@Temperature 18.0 - 28.0 °C
Ultimate, In plane, Dry; EN6031
 
Thermal PropertiesOriginal ValueComments
CTE, linear 30.6 µin/in-°F
@Temperature -50.0 - 20.0 °C
 38.9 µin/in-°F
@Temperature 20.0 - 100 °C
 47.2 µin/in-°F
@Temperature 100 - 180 °C
Glass Transition Temp, Tg -15.0 °Cmidpoint
 205 °COnset
 245 °CPeak
 
Processing PropertiesOriginal ValueComments
Gel Time 20.0 min
@Temperature 180 °C
Time to reach 1000 mPa.s
 20.0 min
@Temperature 180 °C
Time to reach 200 mPa.s
 25.0 min
@Temperature 180 °C
G’ & G’’ crossover
 25.0 min
@Temperature 170 °C
Time to reach 200 mPa.s
 30.0 min
@Temperature 170 °C
Time to reach 1000 mPa.s
 35.0 min
@Temperature 170 °C
G’ & G’’ crossover
 35.0 min
@Temperature 160 °C
Time to reach 200 mPa.s
 40.0 min
@Temperature 160 °C
Time to reach 1000 mPa.s
 45.0 min
@Temperature 150 °C
Time to reach 200 mPa.s
 50.0 min
@Temperature 160 °C
G’ & G’’ crossover
 55.0 min
@Temperature 150 °C
Time to reach 1000 mPa.s
 70.0 min
@Temperature 140 °C
Time to reach 200 mPa.s
 75.0 min
@Temperature 150 °C
G’ & G’’ crossover
 80.0 min
@Temperature 140 °C
Time to reach 1000 mPa.s
 95.0 min
@Temperature 130 °C
Time to reach 200 mPa.s
 110 min
@Temperature 140 °C
G’ & G’’ crossover
 120 min
@Temperature 130 °C
Time to reach 1000 mPa.s
 135 min
@Temperature 120 °C
Time to reach 200 mPa.s
 165 min
@Temperature 130 °C
G’ & G’’ crossover
 170 min
@Temperature 120 °C
Time to reach 1000 mPa.s
 200 min
@Temperature 110 °C
Time to reach 200 mPa.s
 260 min
@Temperature 120 °C
G’ & G’’ crossover
 260 min
@Temperature 110 °C
Time to reach 1000 mPa.s
 290 min
@Temperature 100 °C
Time to reach 200 mPa.s
 345 min
@Temperature 90.0 °C
Time to reach 200 mPa.s
 410 min
@Temperature 110 °C
G’ & G’’ crossover
 410 min
@Temperature 100 °C
Time to reach 1000 mPa.s
 585 min
@Temperature 90.0 °C
Time to reach 1000 mPa.s
 690 min
@Temperature 100 °C
G’ & G’’ crossover
 840 min
@Temperature 80.0 °C
Time to reach 1000 mPa.s
 >= 900 min
@Temperature 70.0 °C
G’ & G’’ crossover
 >= 900 min
@Temperature 80.0 °C
G’ & G’’ crossover
 >= 900 min
@Temperature 90.0 °C
G’ & G’’ crossover
 >= 900 min
@Temperature 70.0 °C
Time to reach 1000 mPa.s
Shelf Life 12.0 Month
@Temperature -18.0 °C
After mixing
 12.0 Month
@Temperature 25.0 °C
Before mixing

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHEXCB9193 / 322349

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.