MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Plastcom SLOVALEN EH 96 FRD 2 PP, flame retardant
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Flame Retardant

Material Notes: Features

Determined for environment, where contact with water is possible, because the electric properties do not change by conditioning. Application - terminals, coil forms, guides in washing machines, tea-pots, dish-washers. Delivered in natural mode and in the full RAL colour scale. Modified homopolymer PP, retarded type with halogen flame retardant. Fulfills basic electric properties: flammability in accordance with UL 94 V2 and 850°C glow wire.

Packaging, transport, stocking

The product is packed in hermetically closed thick-walled 25 kg PE bags, on a 1.000 kg palette coated in a stretch foil, in big bags with a thick PE foil fixed on a 1.000 kg palette, in paper octabins with a thick PE foil fixed on a 1.000 kg palette or in other packaging according to customer requirements. The transport is provided in closed-up vehicles where the material is protected against movement and mechanical damage. The product requires stocking in closed-up, dry places protected against sun and thermal radiation.

Information Provided by Plastcom spol. s r.o.

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.01 g/cc
Linear Mold Shrinkage 0.0238 cm/cm
Linear Mold Shrinkage, Transverse 0.0217 cm/cm
Melt Flow 15 g/10 min
@Load 0.325 kg,
Temperature 270 °C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 18.0 MPa
Elongation at Break 33 %
Tensile Modulus 1200 MPa
Flexural Strength 21.0 MPa
Flexural Modulus 900 MPa
Charpy Impact Unnotched 45.0 kJ/m²
@Temperature -20.0 °C
 NB
@Temperature 23.0 °C
Charpy Impact, Notched 6.00 kJ/m²
@Temperature -20.0 °C
 10.0 kJ/m²
@Temperature 23.0 °C
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+14 ohm-cm
Surface Resistance 1.00e+16 ohm
Dielectric Strength 28.0 kV/mm
Comparative Tracking Index 500 V
 
Thermal PropertiesOriginal ValueComments
Melting Point 130 °C
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °C
Vicat Softening Point 100 °CB
Flammability, UL94 V-2
Glow Wire Test 850 °C
 
Processing PropertiesOriginal ValueComments
Melt Temperature 170 - 190 °C
Mold Temperature 30.0 - 50.0 °C
Injection Pressure 50.0 - 80.0 MPa

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Total PPR LX5 02-15 Polypropylene, Metallocene Film Resin
Lushan M-10H Adhesive Resin for Multi-layer Sausage Casing film
Lushan M-10D Adhesive Resin for Multi-layer Sausage Casing film
Lushan M-10A Adhesive Resin for Multi-layer Sausage Casing film
LG Chemical SEETEC M1425 Polypropylene Impact Copolymer

PPLACO240 / 120864

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.