MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Kalrez® Spectrum™ 0090 Fluoroelastomer  (discontinued **)
Categories: Polymer; Thermoset; Fluoropolymer, TS; Thermoset Fluoroelastomer; Rubber or Thermoset Elastomer (TSE)

Material Notes: DuPont™ Kalrez® 0090 perfluoroelastomer parts deliver durable, reliable sealing solutions for applications requiring excellent rapid gas decompression (RGD) properties as well as high hardness and high modulus properties. Some application areas include downhole equipment such as drilling and completion tools as well as industrial equipment including pumps and valves. Kalrez® 0090 has been certified by two independent labs (see Table 2) to meet rigorous requirements for resistance to RGD. In addition to demonstrated RGD resistance, DuPont™ Kalrez® 0090 seals have other chemical and temperature properties that provide superior performance.

Chemical resistance: Kalrez® parts withstand attack by more than 1800 chemical substances. Kalrez® 0090 can be resistant to sour multi-phase fluids containing H2S as shown by the external NORSOK M-710 Rev 2 Sour Fluid ageing resistance certification provided by MERL (UK).

Broad temperature capability: Kalrez® 0090 retains high levels of resilience up to temperatures as high as 250 °C (482 °F) and down to –21 °C (–5.8 °F). Under pressurized sealing conditions, Kalrez® 0900 has demonstrated low temperature performance down to –40 °C (–40 °F) in customer laboratory tests.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 95ASTM D2240
Tensile Strength at Break 19.49 MPaASTM D412
Elongation at Break 80 %ASTM D412
50% Modulus 0.01418 GPa
@Strain 50 %
ASTM D412
Compression Set 19 %
@Temperature 200 °C,
Time 252000 sec
Pellets; ASTM D395B
 33 %
@Temperature 200 °C,
Time 252000 sec
O-rings; ASTM D395B
 35 %
@Temperature 250 °C,
Time 1.21e+6 sec
O-rings; ASTM D395B
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 250 °CDuPont Test Method
Minimum Service Temperature, Air -21.0 °CDuPont Test Method
 -7.40 °CRetraction Temperature, Tr10; ASTM D1329
Glass Transition Temp, Tg -1.00 °CDuPont Test Method
 
Descriptive Properties
ColorBlack

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Kalrez® 6230 FFKM Perfluoroelastomer
Nitrile Rubber (NBR, Acrylonitrile-Butadiene Rubber)
Mallard Creek Polymers Rovene® 5499 Carboxylated Styrene-Butadiene Emulsion
Overview of materials for Silicone Rubber
Sea-cure (SC-1) Ferritic Stainless Steel (UNS S44660)

PDVC9786 / 170427

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.