MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Meldin Supplier

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Vespel® SP-1 ISO Polyimide
Categories: Polymer; Thermoplastic; Polyimide, Thermoplastic

Material Notes: Parts and stock shapes from unfilled PI (polyimide) resin for high purity and high temperature environments

Information provided by DuPont. This product line has remained with DuPont after the DuPont-Dow merger.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.43 g/ccASTM D 792
Water Absorption 0.24 %Immersion 24h; ASTM D 570
 0.72 %
@Temperature 50.0 °C
Immersion 48h; ASTM D 570
Moisture Absorption at Equilibrium 1.0 - 1.3 %50% RH; ASTM D 570
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell E 45 - 60ASTM D 785
Tensile Strength, Ultimate 41.0 MPa
@Temperature 260 °C
ASTM D 638
 86.0 MPa
@Temperature 23.0 °C
ASTM D 638
Elongation at Break 6.0 %
@Temperature 260 °C
ASTM D 638
 7.5 %
@Temperature 23.0 °C
ASTM D 638
Flexural Strength 62.0 MPa
@Temperature 260 °C
ASTM D 790
 110 MPa
@Temperature 23.0 °C
ASTM D 790
Flexural Modulus 1723 MPa
@Temperature 260 °C
ASTM D 790
 3101 MPa
@Temperature 23.0 °C
ASTM D 790
Shear Strength 90.0 MPaASTM D 732
Izod Impact, Notched 0.427 J/cm
@Temperature 23.0 °C
ASTM D 256
Izod Impact, Unnotched 747.0 J/m
@Temperature 23.0 °C
ASTM D 4812
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 8.00e+16 ohm-cmASTM D 257
Surface Resistance 4.00e+12 ohmASTM D 257
Dielectric Constant 3.66
@Frequency 1e+6 Hz,
Temperature 23.0 °C
ASTM D 150
 3.73
@Frequency 10000 Hz,
Temperature 23.0 °C
ASTM D 150
 3.74
@Frequency 100 Hz,
Temperature 23.0 °C
ASTM D 150
Dielectric Strength 24.6 kV/mm
@Thickness 2.00 mm,
Temperature 23.0 °C
Short time; ASTM D149
Dissipation Factor 0.0015
@Frequency 100 Hz
ASTM D 150
 0.0050
@Frequency 1e+6 Hz
ASTM D 150
 0.0054
@Frequency 10000 Hz
ASTM D 150
Comparative Tracking Index 175 - 249 VIEC 60112
 175 - 249 V
@Thickness 3.00 mm
UL 746A
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 360 °CASTM D 648
UL RTI, Electrical 130 °C
@Thickness 0.750 mm
UL 746B
 130 °C
@Thickness 1.70 mm
UL 746B
 130 °C
@Thickness 3.00 mm
UL 746B
UL RTI, Mechanical with Impact 130 °C
@Thickness 1.70 mm
UL 746B
 130 °C
@Thickness 0.750 mm
UL 746B
 130 °C
@Thickness 3.00 mm
UL 746B
UL RTI, Mechanical without Impact 130 °C
@Thickness 0.750 mm
UL 746B
 130 °C
@Thickness 1.70 mm
UL 746B
 130 °C
@Thickness 3.00 mm
UL 746B
Flammability, UL94 V-0
@Thickness 1.70 mm
IEC 60695-11-10
 V-0
@Thickness 0.750 mm
IEC 60695-11-10
 V-0
@Thickness 0.750 mm
UL94
 V-0
@Thickness 1.70 mm
UL94
 V-0
@Thickness 3.00 mm
IEC 60695-11-10
 V-0
@Thickness 3.00 mm
UL94
 5VA
@Thickness 0.750 mm
IEC 60695-11-20
Oxygen Index 53 %ASTM D 2863
 
Descriptive Properties
Contains Flame RetardantYes
Heat StabilizedYes
Polymer FamilyPolyimide
Polymer TypePI
Region AvailableAmericas
 Asia/Pacific
 Europe

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Vespel® SP-1 Polyimide, Machined
DuPont Mobility and Materials Vespel® SP-1 Polyimide, Direct formed
DuPont Mobility and Materials Vespel® SP-22 DF Polyimide
Mitsubishi Chemical Advanced Materials Semitron® MDS 100 (ASTM Product Data Sheet)
DuPont Mobility and Materials Vespel® SP-21 Polyimide, 15% Graphite Filled, Direct formed

PDTA7752 / 89864

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.