MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Rynite® RE5264E NC010 PET-GF36  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polyethylene Terephthalate (PET); Polyethylene Terephthalate (PET), 40% Glass Reinforced

Material Notes:

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.66 g/ccISO 1183
Linear Mold Shrinkage, Flow 0.0010 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.010 cm/cmnormal; ISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 200 MPaISO 527-1/-2
Elongation at Break 2.4 %ISO 527-1/-2
Tensile Modulus 14000 MPaISO 527-1/-2
Flexural Strength 280 MPaISO 178
Flexural Modulus 12000 MPaISO 178
Poissons Ratio 0.33
Charpy Impact Unnotched 60.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 9.50 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 21.5 kV/mmIEC 60243-1
 
Thermal PropertiesOriginal ValueComments
Melting Point 247 °C10°C/min; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 230 °CISO 75-1/-2
 
Processing PropertiesOriginal ValueComments
Melt Temperature 285 °COptimum, Injection
 280 - 300 °CInjection
Mold Temperature 120 - 140 °CInjection
 140 °COptimum, Injection
Ejection Temperature 170 °C
Drying Temperature 120 °C
@Time 14400 - 21600 sec
Injection; Dehumidified Dryer
Moisture Content 0.010 %At levels above 0.01%, strength and toughness will decrease, even though parts may not exhibit surface defects.
Hold Pressure 80.0 MPaInjection
 
Descriptive Properties
AdditivesRelease agent
Delivery formPellets
Drying Recommendedyes
Hold pressure time (s/mm)4Injection
Injection Back PressureAs low as possible
Max. screw tangential speed (m/s)0.2
Part Marking Code>PET-GF36<ISO 11469
ProcessingInjection Molding
Regional AvailabilityEurope
 Near East/Africa
Resin IdentificationPET-GF36ISO 1043

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PDSX5279c / 254448

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.