MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Extreme Materials from MCAM
Visit Mitsubishi Chemical Advanced Materials for Extreme Materials - high performance plastic machining stock engineered to replace metals such as nickel alloys or stainless steel.

(Viewing data as-entered. Click here to return)
ATI Allegheny Ludlum AL 825™ Nickel Alloy
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Allegheny Ludlum AL 825 alloy is an austenitic nickel-iron-chromium-molybdenum-copper alloy containing high levels of corrosion resistance to both moderately oxidizing and moderately reducing environments. The alloy has a high level of nickel, which in combination with the level of molybdenum and copper, produces substantially improved corrosion resistance in reducing environments compared to the standard stainless steels.

The nickel content is sufficiently high to provide good resistance to chloride stress corrosion cracking. The chromium and molybdenum content of the alloy provides a level of resistance to chloride ion pitting, however, not to the level of other Allegheny Ludlum alloys. In addition, the alloy is stabilized against sensitization in the welded condition by the addition of a specified level of titanium. Because of this stabilization, the material is resistant to intergranular attack after exposure in the temperature range which would sensitize unstabilized stainless steels.

This alloy has a long history of use in many corrosive environments and has been incorporated in ASTM and ASME specifications for many years.

Information provided by Allegheny Ludlum

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.13 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 85Typical Annealed
Tensile Strength, Ultimate 690 MPatypical
Tensile Strength, Yield 300 MPatypical
Elongation at Break 45 %typical in 2"
Modulus of Elasticity 195 GPatypical
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000113 ohm-cm
Magnetic Permeability <= 1.02
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.9 µm/m-°C
@Temperature 20.0 - 93.0 °C
 15.3 µm/m-°C
@Temperature 20.0 - 315 °C
 15.7 µm/m-°C
@Temperature 20.0 - 427 °C
Specific Heat Capacity 0.500 J/g-°C
Maximum Service Temperature, Air 538 °CDuctility maintained well above this temp.
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.15 %
Carbon, C 0.020 %
Chromium, Cr 21 %
Copper, Cu 2.0 %
Iron, Fe 32.053 %as balance
Manganese, Mn 0.50 %
Molybdenum, Mo 3.0 %
Nickel, Ni 40 %
Phosphorus, P 0.025 %
Silicon, Si 0.25 %
Sulfur, S 0.0020 %
Titanium, Ti 1.0 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Austenitic
416 Stainless Steel, annealed wire 6.4 mm diameter
416 Stainless Steel, tempered and cold drawn bar 25 mm diameter
416 Stainless Steel, annealed bar
ATI Allegheny Ludlum Stainless Steel Free Machining Grade Type 416, Tempered at 704°C (UNS S41600)

NLN825 / 18026

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.