MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Kaiser 6040 T8 Rod & Bar
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 6000 Series Aluminum Alloy

Material Notes: 6040 is a lead-free alternative to 6262. The alloy offers very good machinability along with good corrosion resistance. It also has excellent coating acceptance (anodize response). It can be used in place of 6062. Physical and mechanical properties are equivalent to 6262.

  • Ratings A through E are relative ratings in decreasing order of merit, based on exposures to sodium chloride solution by intermittent spraying or immersion. Alloys with A and B ratings can be used in industrial and seacoast atmospheres without protection. Alloys with C, D and E ratings generally should be protected at least on faying surfaces.
  • Stress-corrosion cracking ratings are based on service experience and laboratory tests of specimens exposed to the 3.5% sodium chloride alternate immersion test.
    A= No known instance of failure in service or in laboratory tests.
    B= No known instance of failure in service; limited failures in laboratory tests of short transverse specimens.
    C= Service failures with sustained tension stress acting in short transverse direction relative to grain structure; limited failures in laboratory tests of long transverse specimens.
    D= Limited service failures with sustained longitudinal or long transverse
  • Ratings A through D for Workability (cold), A through E for Machinability and A through C for Anodize Response, are relative ratings in decreasing order of merit.
  • Ratings A through D for Weldability and Brazeability are relative ratings defined as follows:
    A= Generally weldable by all commercial procedures and methods.
    B= Weldable with special techniques or for specific applications that justify preliminary trials or testing to develop welding procedure and weld performance.
    C= Limited weldability because of crack sensitivity or loss in resistance to corrosion and mechanical properties.
    D= No commonly used welding methods have been developed.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.70 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 62100 kg 1/16" Ball
Tensile Strength, Ultimate 324 MPa
@Diameter 12.7 mm
Tensile Strength, Yield 303 MPa
@Diameter 12.7 mm
Elongation at Break 14 %
@Diameter 12.7 mm
4D
Shear Strength 207 MPaUltimate
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 93.75 - 98.15 %As Balance
Bismuth, Bi 0.15 - 0.70 %
Chromium, Cr <= 0.15 %
Copper, Cu 0.20 - 0.80 %
Iron, Fe <= 0.70 %
Magnesium, Mg 0.80 - 1.2 %
Manganese, Mn <= 0.15 %
Other, each <= 0.050 %
Other, total <= 0.15 %
Silicon, Si 0.40 - 0.80 %
Tin, Sn 0.30 - 1.2 %
Titanium, Ti <= 0.15 %
Zinc, Zn <= 0.25 %
 
Descriptive Properties
Anodize Response3A
Cold Workability3D
General Corrosion Resistance1B
Machinability3B
Stress Corrosion Resistance2A

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Kaiser 7068 T6, T6511 Rod & Bar
Aluminum 6061-T6; 6061-T651
Aluminum 6053-T6
Aluminum 6053-O
Alclad Aluminum 6061-T6, T651

NKAISER8 / 17668

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.