MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SABIC LNP™ LUBRICOMP™ Compound KA000M Acetal (POM) Copolymer
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: LNP LUBRICOMP KA000M compound is based on POM (Acetal) resin containing aramid powder and proprietary lubricant. Added features of this grade include: Internally Lubricated, Wear Resistant.

Features: Internally Lubricated,Wear resistant

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.35 g/ccISO 1183
Water Absorption 0.20 - 0.40 %
@Time 86400 sec
ASTM D570
 0.20 - 0.40 %
@Time 86400 sec
ISO 62-1
Moisture Absorption 0.200 - 0.300 %23°C/50% RH/24 hrs; ASTM D570
 0.200 - 0.300 %23°C / 50% RH; ISO 62
Viscosity 4.0 - 6.0 cP
@Load 2.16 kg,
Temperature 190 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.015 - 0.025 cm/cmSABIC method
Linear Mold Shrinkage, Transverse 0.015 - 0.025 cm/cmSABIC method
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 42.0 MPa5 mm/min; ASTM D638
 42.0 MPa5 mm/min; ISO 527
Elongation at Break 6.0 %5 mm/min; ASTM D638
 7.8 %5 mm/min; ISO 527
Elongation at Yield 5.3 %5 mm/min; ASTM D638
 6.0 %5 mm/min; ISO 527
Tensile Modulus 2600 MPa5 mm/min; ASTM D638
 2600 MPa1 mm/min; ISO 527
Flexural Strength 70.0 MPayield, 2 mm/min; ISO 178
 74.0 MPa1.3 mm/min, 50 mm span; ASTM D790
 22.0 MPa
@Temperature 100 °C
yield, 2 mm/min; ISO 178
 42.0 MPa
@Temperature 60.0 °C
yield, 2 mm/min; ISO 178
Flexural Modulus 2400 MPa2 mm/min; ISO 178
 2600 MPa1.3 mm/min, 50 mm span; ASTM D790
 800 MPa
@Temperature 100 °C
2 mm/min; ISO 178
 1400 MPa
@Temperature 60.0 °C
2 mm/min; ISO 178
Flexural Strain at Break 7.0 %2 mm/min; ISO 178
 7.0 %
@Temperature 60.0 °C
2 mm/min; ISO 178
 7.0 %
@Temperature 100 °C
2 mm/min; ISO 178
Izod Impact Notched 28.0 JASTM D256
Izod Impact, Unnotched 310 J/mASTM D4812
Izod Impact, Notched (ISO) 3.00 kJ/m²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 25.0 kJ/m²80*10*4; ISO 180/1U
Charpy Impact Unnotched 30.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 2.00 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
Coefficient of Friction, Dynamic 0.20ASTM D3702 Modified: Manual
Coefficient of Friction, Static 0.22ASTM D3702 Modified: Manual
K (wear) Factor 9.00 x 10-10 in³-min/ft-lb-hrWasher; ASTM D3702 Modified: Manual
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 120 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 130 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 150 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi) 90.0 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 96.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 143 °CRate B/50; ASTM D1525
 143 °CRate B/50; ISO 306
 144 °CRate B/120; ISO 306
Flammability, UL94 HB
@Thickness >=1.50 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Zone 2 195 - 205 °C
Zone 3 210 - 220 °C
Melt Temperature 200 - 215 °CInjection Molding
Mold Temperature 80.0 - 110 °C
Drying Temperature 80.0 °CInjection Molding
Dry Time 4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH80819 / 288766

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.