MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Idemitsu Kosan TARFLON™ LC1500 Polycarbonate, Optical Grade
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Optical Grade

Material Notes: Light guiding Standard. LC1500 has been used widely in LCD backlight parts and automotive daylight running lamp (DRL).

General Tarflon™ Information: Polycarbonate is known for its high impact resistance, good transparency and heat resistance, and superb precision and electrical properties. TARFLON is used in wide range of applications such as housewares, office equipment , mobile devices, communications equipment , display devices such as LCD backlight parts, automotive , lighting and many fields.

Information provided by Idemitsu Losan Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.20 g/ccISO 1183(JIS K7112)
Moisture Absorption 0.230 %
@Time 86400 sec
50% RH; ISO 62(JIS K7209)
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cmIdemitsu Method
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cmIdemitsu Method
Melt Flow 78 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ISO 1133 (JIS K7210)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 50ISO 2039-2 (JIS K7202-2)
Hardness, Rockwell R 120ISO 2039-2 (JIS K7202-2)
Tensile Strength, Yield 65.0 MPaISO 527-1,2 (JIS K7161, 7162)
Elongation at Break 80 %ISO 527-1,2 (JIS K7161, 7162)
Flexural Strength 90.0 MPaISO 178 (JIS K7171)
Flexural Modulus 2.30 GPaISO 178 (JIS K7171)
Charpy Impact, Notched 15.0 kJ/m²ISO 179-1 (JIS K7111)
 
Thermal PropertiesOriginal ValueComments
CTE, linear 65.0 µm/m-°CISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 127 °CISO 75-1,2 (JIS K7191-1,2)
UL RTI, Electrical 80.0 °CUL746B
UL RTI, Mechanical with Impact 80.0 °CUL746B
UL RTI, Mechanical without Impact 80.0 °CUL746B
Flammability, UL94 V-2
@Thickness 0.400 mm
NC
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.585ASTM D542
Transmission, Visible 90 %Total Luminous; ISO 13468-1 (JIS K7361-1)
 
Processing PropertiesOriginal ValueComments
Melt Temperature 240 - 260 °CCylinder Temperature
Mold Temperature 80.0 - 120 °C
Drying Temperature 120 °C
@Time 18000 - 28800 sec

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PIDEM256 / 249620

Rulon Bearings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.