MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Kolon CT503 Super Clear Film  (discontinued **)
Categories: Polymer; Film

Material Notes: CT Series is Hyper transparency product with acryl type slippery solvent coated on single or both sides. Specially developed to maximize adhesive strength to many different kind of solvents.

Applications: Label, Window, High-gloss Metallizing, Paper Lamination, Transfer, Hologram

Information provided by Kolon

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Surface Tension 38 dynes/cmInside; ASTM D2578
 38 dynes/cmInside; ASTM D2578
 38 dynes/cmInside; ASTM D2578
 52 dynes/cmInside; ASTM D2578
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 160 %
@Thickness 0.230 mm
ASTM D882
 210 %
@Thickness 0.100 mm
ASTM D882
 210 %
@Thickness 0.750 mm
ASTM D882
 230 %
@Thickness 0.125 mm
ASTM D882
Film Elongation at Break, TD 130 %
@Thickness 0.125 mm
ASTM D882
 140 %
@Thickness 0.100 mm
ASTM D882
 140 %
@Thickness 0.750 mm
ASTM D882
 140 %
@Thickness 0.230 mm
ASTM D882
Coefficient of Friction, Dynamic <= 0.50
@Thickness 0.230 mm
ASTM D1894
 <= 0.70
@Thickness 0.750 mm
ASTM D1894
 <= 0.70
@Thickness 0.100 mm
ASTM D1894
 <= 0.70
@Thickness 0.125 mm
ASTM D1894
Coefficient of Friction, Static <= 0.45
@Thickness 0.230 mm
ASTM D1894
 <= 0.70
@Thickness 0.125 mm
ASTM D1894
 <= 0.70
@Thickness 0.100 mm
ASTM D1894
 <= 0.70
@Thickness 0.750 mm
ASTM D1894
Film Tensile Strength at Break, MD 176 MPa
@Thickness 0.125 mm
ASTM D882
 186 MPa
@Thickness 0.750 mm
ASTM D882
 196 MPa
@Thickness 0.100 mm
ASTM D882
 245 MPa
@Thickness 0.230 mm
ASTM D882
Film Tensile Strength at Break, TD 186 MPa
@Thickness 0.125 mm
ASTM D882
 206 MPa
@Thickness 0.100 mm
ASTM D882
 206 MPa
@Thickness 0.750 mm
ASTM D882
 245 MPa
@Thickness 0.230 mm
ASTM D882
 
Thermal PropertiesOriginal ValueComments
Shrinkage, MD 0.70 %
@Thickness 0.100 mm
Heat Shrinkage; ASTM D2305
 0.70 %
@Thickness 0.750 mm
Heat Shrinkage; ASTM D2305
 1.0 %
@Thickness 0.125 mm
Heat Shrinkage; ASTM D2305
 1.5 %
@Thickness 0.230 mm
Heat Shrinkage; ASTM D2305
Shrinkage, TD 0.00 %
@Thickness 0.230 mm
Heat Shrinkage; ASTM D2305
 0.20 %
@Thickness 0.750 mm
Heat Shrinkage; ASTM D2305
 0.20 %
@Thickness 0.125 mm
Heat Shrinkage; ASTM D2305
 0.70 %
@Thickness 0.100 mm
Heat Shrinkage; ASTM D2305
 
Optical PropertiesOriginal ValueComments
Haze <= 0.50 %
@Thickness 0.230 mm
ASTM D1003
 <= 1.0 %
@Thickness 0.750 mm
ASTM D1003
 <= 1.0 %
@Thickness 0.100 mm
ASTM D1003
 <= 1.4 %
@Thickness 0.125 mm
ASTM D1003
 
Descriptive Properties
Surface Roughness, Ra1.4 nmOutside; Coating on PET film
 4.8 nmInside; Coating on PET film

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PKOKZ822 / 185365

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.