MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Borealis Borcycle™ NAV101L Recycled LDPE
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE)

Material Notes: Borcycle NAV101L belongs to the Borcycle" M grade portfolio. It is a 100% post-consumer, transparent, gel-reduced Low Density Polyethylene recyclate (rLDPE) supplied in pellet form for high-end blown film applications. NAV101L is an ideal LDPE used where sustainability and circularity matter. NAV101L is a 100% post-consumer recyclate including a large part of recycled post-consumer plastic waste coming from pre-sorted municipal (household) waste. NAV101L is part of EuCertPlast certificate according to European Standard EN 15343:2007 (certificate available upon request). Due to the nature of recyclates, some variation in color can be observed between batches. Cas No. 9002-88-4

Typical characteristics:

  • High transparency with reduced gel content
  • Available in homogenized 24-ton truckloads
  • Low odor
  • Filtration: 60 µm
Applications:
  • Collation shrink film
  • Shrink film
  • Lamination films for non-food contact primary packaging
  • Non-food contact primary packaging
  • Secondary and tertiary packaging where transparency and reduced gel content are key parameters

Information provided by Borealis AG

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.490 g/ccISO 60
Density 0.925 g/ccISO 1183-1
Melt Flow 0.750 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ISO 1133-1
Storage Temperature <= 50.0 °C
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 230 %ISO 527-3
Film Elongation at Break, TD 530 %ISO 527-3
Tensile Modulus 215 MPaMD; ISO 527-3
 255 MPaTD; ISO 527-3
Elmendorf Tear Strength MD 1.60 gISO 6383-2
Elmendorf Tear Strength TD 4.30 gISO 6383-2
Dart Drop Test 75.0 gISO 7765-1
Film Tensile Strength at Break, MD 15.0 MPaISO 527-3
Film Tensile Strength at Break, TD 16.0 MPaISO 527-3
 
Optical PropertiesOriginal ValueComments
Haze 29.0 %ASTM D1003
Gloss 35.0 %45°; ASTM D2457
 
Processing PropertiesOriginal ValueComments
Melt Temperature 160 - 190 °C
Moisture Content <= 0.0500 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBORE9641 / 322998

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.