MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
SABIC LNP™ THERMOCOMP™ Compound D151RC Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LNP THERMOCOMP D151RC compound is based on recycled Polycarbonate (PC) resin containing 10% glass fiber. Added features of this grade include: High Modulus, Good Surface, Low Warpage, Good Ductility, Non-Brominated & Non-Chlorinated Flame Retardant. Post-Consumer Recycling (PCR) Polycarbonate content up to 35%.

Features: Post-Consumer Recycled (PCR) content,High Stiffness,Enhanced Ductility,Flame Retardant,Non-Chlorinated,Non-Brominated,Low Warpage,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.27 g/ccASTM D792
Water Absorption 0.040 %
@Time 86400 sec
ISO 62-1
Moisture Absorption 0.0200 %Injection Molding
Viscosity 11 cP
@Load 1.20 kg,
Temperature 300 °C
MVR cc/10 min; ISO 1133
 23 cP
@Load 2.16 kg,
Temperature 300 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cm24hrs; ASTM D955
Linear Mold Shrinkage, Transverse 0.0030 - 0.0050 cm/cm24hrs; ASTM D955
Melt Flow 12 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 24 g/10 min
@Load 2.16 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 82.0 MPa5 mm/min; ASTM D638
 82.0 MPa5 mm/min; ISO 527
Elongation at Break 3.6 %5 mm/min; ISO 527
 3.7 %5 mm/min; ASTM D638
Tensile Modulus 4380 MPa1 mm/min; ISO 527
 4430 MPa5 mm/min; ASTM D638
Flexural Strength 130 MPabrk, 1.3 mm/min, 50 mm span; ASTM D790
 132 MPabreak, 2mm/min; ISO 178
 133 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
 134 MPayield, 2 mm/min; ISO 178
Flexural Modulus 4070 MPa1.3 mm/min, 50 mm span; ASTM D790
 4180 MPa2 mm/min; ISO 178
Izod Impact Notched 140 JASTM D256
 75.0 J
@Temperature -30.0 °C
ASTM D256
Izod Impact, Unnotched 700 J/mASTM D4812
Izod Impact, Notched (ISO) 13.0 kJ/m²80*10*4; ISO 180/1A
 7.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 42.0 kJ/m²80*10*4; ISO 180/1U
Dart Drop, Total Energy 21.0 JASTM D3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+16 ohm-cmASTM D257
Surface Resistance >= 1.00e+16 ohmASTM D257
Dielectric Constant 3.03
@Frequency 1.10e+9 Hz
SABIC method
 3.04
@Frequency 1.90e+9 Hz
SABIC method
 3.05
@Frequency 5.00e+9 Hz
SABIC method
 3.05
@Frequency 1e+10 Hz
SABIC method
Dissipation Factor 0.0062
@Frequency 5.00e+9 Hz
SABIC method
 0.0063
@Frequency 1.90e+9 Hz
SABIC method
 0.0064
@Frequency 1.10e+9 Hz
SABIC method
 0.0064
@Frequency 1e+10 Hz
SABIC method
Comparative Tracking Index 175 - 250 VUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 35.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 40.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ASTM E831
CTE, linear, Transverse to Flow 69.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 83.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 121 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 121 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 115 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 115 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 123 °CRate B/50; ISO 306
 126 °CRate B/120; ISO 306
UL RTI, Electrical 80.0 °CUL 746B
UL RTI, Mechanical with Impact 80.0 °CUL 746B
UL RTI, Mechanical without Impact 80.0 °CUL 746B
Flammability, UL94 V-2
@Thickness >=0.500 mm
UL 94
 V-0
@Thickness >=0.600 mm
UL 94
Glow Wire Ignition Temperature 850 °C
@Thickness 1.00 mm
IEC 60695-2-13
 850 °C
@Thickness 1.60 mm
IEC 60695-2-13
 850 °C
@Thickness 2.00 mm
IEC 60695-2-13
Glow Wire Flammability Index 960 °C
@Thickness 1.00 mm
IEC 60695-2-12
 960 °C
@Thickness 1.60 mm
IEC 60695-2-12
 960 °C
@Thickness 2.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 285 - 305 °C
Zone 2 270 - 290 °C
Zone 3 280 - 300 °C
Melt Temperature 285 - 310 °CInjection Molding
Mold Temperature 80.0 - 110 °C
Drying Temperature 110 °CInjection Molding
Dry Time 3.00 - 6.00 hourInjection Molding
Back Pressure 0.100 - 0.300 MPa
Screw Speed 50 - 90 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH81480 / 289427

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.