MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Overview of materials for Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polybutylene Terephthalate (PBT), 20% Glass Fiber Filled". Specific grades with glass content between 15% and 24% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.22 - 1.80 g/ccAverage value: 1.46 g/cc Grade Count:331
 1.14 - 1.32 g/cc
@Temperature 205 - 250 °C
Average value: 1.20 g/cc Grade Count:8
Filler Content 15.0 - 20.0 %Average value: 16.9 % Grade Count:86
Water Absorption 0.0100 - 0.500 %Average value: 0.213 % Grade Count:123
Moisture Absorption at Equilibrium 0.0200 - 0.400 %Average value: 0.150 % Grade Count:126
Water Absorption at Saturation 0.150 - 0.500 %Average value: 0.345 % Grade Count:23
Viscosity 150000 cPAverage value: 150000 cP Grade Count:3
 17.0 - 18.0 cP
@Temperature 250 - 265 °C
Average value: 45700 cP Grade Count:3
 17.0 - 18.0 cP
@Load 5.00 - 5.00 kg
Average value: 45700 cP Grade Count:3
 9.00 - 460190 cP
@Shear Rate 10.0 - 100000 1/s
Average value: 45700 cP Grade Count:6
 9.00 - 460190 cP
@Temperature 230 - 280 °C
Average value: 45700 cP Grade Count:6
Viscosity Test 69.0 - 116 cm³/gAverage value: 91.5 cm³/g Grade Count:10
Viscosity Number 94.0 - 135 cm³/gAverage value: 107 cm³/g Grade Count:19
Maximum Moisture Content 0.0200 - 0.0400Average value: 0.0209 Grade Count:22
 0.200 - 0.200
@Temperature 120 - 120 °C
Average value: 0.200 Grade Count:1
 0.200 - 0.200
@Time 299 - 299 sec
Average value: 0.200 Grade Count:1
Linear Mold Shrinkage 0.00100 - 0.0200 cm/cmAverage value: 0.00603 cm/cm Grade Count:235
 0.00400 - 0.00400 cm/cm
@Temperature 80.0 - 80.0 °C
Average value: 0.00367 cm/cm Grade Count:2
 0.00300 - 0.00400 cm/cm
@Temperature 260 - 260 °C
Average value: 0.00367 cm/cm Grade Count:2
 0.00300 - 0.00400 cm/cm
@Pressure 60.0 - 60.0 MPa
Average value: 0.00367 cm/cm Grade Count:2
Linear Mold Shrinkage, Transverse 0.00100 - 0.0180 cm/cmAverage value: 0.0107 cm/cm Grade Count:95
 0.0110 - 0.0120 cm/cm
@Temperature 80.0 - 80.0 °C
Average value: 0.0108 cm/cm Grade Count:2
 0.0100 - 0.0110 cm/cm
@Temperature 260 - 260 °C
Average value: 0.0108 cm/cm Grade Count:2
 0.0100 - 0.0110 cm/cm
@Pressure 60.0 - 60.0 MPa
Average value: 0.0108 cm/cm Grade Count:2
Melt Flow 2.00 - 58.0 g/10 minAverage value: 22.4 g/10 min Grade Count:120
Spiral Flow 36.0 - 43.0 cmAverage value: 39.7 cm Grade Count:3
Ash 13.0 - 24.0 %Average value: 17.4 % Grade Count:10
 15.0 - 15.0 %
@Temperature 625 - 625 °C
Average value: 15.0 % Grade Count:1
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 70.0 - 109Average value: 90.2 Grade Count:42
Hardness, Rockwell R 90.0 - 120Average value: 115 Grade Count:33
Ball Indentation Hardness 128 - 200 MPaAverage value: 167 MPa Grade Count:11
Tensile Strength, Ultimate 47.0 - 140 MPaAverage value: 99.8 MPa Grade Count:268
 40.0 - 165 MPa
@Temperature -40.0 - 150 °C
Average value: 79.0 MPa Grade Count:8
Tensile Strength, Yield 62.1 - 125 MPaAverage value: 96.9 MPa Grade Count:80
Elongation at Break 1.00 - 155 %Average value: 5.03 % Grade Count:285
 1.90 - 6.30 %
@Temperature 0.000 - 150 °C
Average value: 4.37 % Grade Count:5
Elongation at Yield 2.00 - 115 %Average value: 11.9 % Grade Count:9
Modulus of Elasticity 3.50 - 14.0 GPaAverage value: 6.58 GPa Grade Count:179
 2.06843 - 6.41212 GPa
@Temperature -40.0 - 150 °C
Average value: 4.22 GPa Grade Count:5
Flexural Yield Strength 86.0 - 190 MPaAverage value: 152 MPa Grade Count:241
 80.0 - 80.0 MPa
@Temperature 90.0 - 90.0 °C
Average value: 80.0 MPa Grade Count:1
Flexural Modulus 3.20 - 10.0 GPaAverage value: 5.66 GPa Grade Count:245
 3.50 - 5.00 GPa
@Temperature 60.0 - 120 °C
Average value: 4.03 GPa Grade Count:2
Flexural Strain at Break 3.00 - 4.50 %Average value: 3.54 % Grade Count:5
Flexural Strain at Yield 3.70 - 4.40 %Average value: 4.06 % Grade Count:5
Poissons Ratio 0.340 - 0.370Average value: 0.351 Grade Count:14
Izod Impact 50.0 JAverage value: 50.0 J Grade Count:3
 50.0 - 50.0 J
@Temperature -30.0 - 0.000 °C
Average value: 50.0 J Grade Count:3
Izod Impact, Notched 0.267 - 1.60 J/cmAverage value: 0.634 J/cm Grade Count:134
 0.430 - 0.600 J/cm
@Temperature -40.0 - -20.0 °C
Average value: 0.570 J/cm Grade Count:5
Izod Impact, Unnotched 0.588 - 8.17 J/cmAverage value: 5.37 J/cm Grade Count:20
 3.30 - 3.60 J/cm
@Temperature -30.0 - -30.0 °C
Average value: 3.52 J/cm Grade Count:4
Izod Impact, Notched (ISO) 3.50 - 60.0 kJ/m²Average value: 8.25 kJ/m² Grade Count:85
 4.00 - 10.0 kJ/m²
@Temperature -40.0 - 30.0 °C
Average value: 7.18 kJ/m² Grade Count:26
Izod Impact, Unnotched (ISO) 12.2 - 65.0 kJ/m²Average value: 44.0 kJ/m² Grade Count:41
 10.5 - 55.0 kJ/m²
@Temperature -40.0 - 30.0 °C
Average value: 33.5 kJ/m² Grade Count:18
Charpy Impact Unnotched 0.450 - 6.90 J/cm²Average value: 4.32 J/cm² Grade Count:121
 1.39 - 6.50 J/cm²
@Temperature -40.0 - -20.0 °C
Average value: 3.77 J/cm² Grade Count:73
Charpy Impact, Notched 0.350 - 2.00 J/cm²Average value: 0.737 J/cm² Grade Count:167
 0.300 - 1.00 J/cm²
@Temperature -40.0 - -20.0 °C
Average value: 0.690 J/cm² Grade Count:76
Dart Drop, Total Energy 5.00 JAverage value: 5.00 J Grade Count:3
Coefficient of Friction 0.150 - 0.200Average value: 0.174 Grade Count:4
Tensile Creep Modulus, 1 hour 3500 - 7300 MPaAverage value: 5600 MPa Grade Count:11
Tensile Creep Modulus, 1000 hours 2400 - 6900 MPaAverage value: 4510 MPa Grade Count:12
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 1.00e+13 - 1.00e+17 ohm-cmAverage value: 1.44e+16 ohm-cm Grade Count:173
Surface Resistance 120 - 3.00e+17 ohmAverage value: 1.02e+16 ohm Grade Count:103
Dielectric Constant 2.70 - 5.20Average value: 3.63 Grade Count:119
Dielectric Strength 14.0 - 100 kV/mmAverage value: 24.8 kV/mm Grade Count:157
Dissipation Factor 0.000700 - 0.150Average value: 0.0167 Grade Count:87
Dielectric Loss Index 0.00200 - 0.0200Average value: 0.0187 Grade Count:14
Arc Resistance 0.000 - 180 secAverage value: 111 sec Grade Count:30
Comparative Tracking Index 125 - 600 VAverage value: 330 V Grade Count:120
Hot Wire Ignition, HWI 7.00 - 120 secAverage value: 36.4 sec Grade Count:8
High Amp Arc Ignition, HAI 30.0 - 120 arcsAverage value: 112 arcs Grade Count:8
High Voltage Arc-Tracking Rate, HVTR 25.4 - 150 mm/minAverage value: 99.5 mm/min Grade Count:5
 
Thermal PropertiesOriginal ValueComments
CTE, linear 20.0 - 110 µm/m-°CAverage value: 40.4 µm/m-°C Grade Count:117
 30.0 - 30.0 µm/m-°C
@Temperature 50.0 - 120 °C
Average value: 30.0 µm/m-°C Grade Count:1
CTE, linear, Transverse to Flow 61.0 - 173 µm/m-°CAverage value: 99.7 µm/m-°C Grade Count:68
 150 - 150 µm/m-°C
@Temperature 50.0 - 120 °C
Average value: 150 µm/m-°C Grade Count:1
Specific Heat Capacity 1.50 - 1.84 J/g-°CAverage value: 1.67 J/g-°C Grade Count:6
 1.85 - 1.90 J/g-°C
@Temperature 205 - 250 °C
Average value: 1.87 J/g-°C Grade Count:5
Thermal Conductivity 0.150 - 0.280 W/m-KAverage value: 0.217 W/m-K Grade Count:9
 0.240 - 0.260 W/m-K
@Temperature 205 - 250 °C
Average value: 0.248 W/m-K Grade Count:5
Melting Point 178 - 255 °CAverage value: 224 °C Grade Count:158
Maximum Service Temperature, Air 75.0 - 330 °CAverage value: 167 °C Grade Count:28
Hot Ball Pressure Test 125 - 215 °CAverage value: 159 °C Grade Count:5
Deflection Temperature at 0.46 MPa (66 psi) 99.0 - 230 °CAverage value: 213 °C Grade Count:217
Deflection Temperature at 1.8 MPa (264 psi) 65.0 - 220 °CAverage value: 194 °C Grade Count:299
Deflection Temperature at 8.0 MPa 65.0 - 140 °CAverage value: 94.4 °C Grade Count:16
Vicat Softening Point 128 - 220 °CAverage value: 206 °C Grade Count:74
Glass Transition Temp, Tg 44.0 - 65.0 °CAverage value: 57.5 °C Grade Count:23
UL RTI, Electrical 50.0 - 140 °CAverage value: 127 °C Grade Count:13
UL RTI, Mechanical with Impact 50.0 - 140 °CAverage value: 121 °C Grade Count:13
UL RTI, Mechanical without Impact 50.0 - 140 °CAverage value: 124 °C Grade Count:13
Flammability, UL94 HB - 5VAGrade Count:292
Flame Spread 24.0 - 100 mm/minAverage value: 45.5 mm/min Grade Count:12
Oxygen Index 19.0 - 35.0 %Average value: 24.7 % Grade Count:37
Glow Wire Test 650 - 960 °CAverage value: 802 °C Grade Count:53
 
Processing PropertiesOriginal ValueComments
Processing Temperature 20.0 - 275 °CAverage value: 184 °C Grade Count:51
Nozzle Temperature 225 - 270 °CAverage value: 250 °C Grade Count:55
Die Temperature 240 - 275 °CAverage value: 257 °C Grade Count:22
Melt Temperature 203 - 280 °CAverage value: 250 °C Grade Count:159
Mold Temperature 30.0 - 130 °CAverage value: 79.9 °C Grade Count:174
Injection Velocity 70.0 - 300 mm/secAverage value: 261 mm/sec Grade Count:16
Drying Temperature 80.0 - 140 °CAverage value: 118 °C Grade Count:141
Moisture Content 0.000 - 0.400 %Average value: 0.0417 % Grade Count:86
Dew Point -40.0 - -28.9 °CAverage value: -29.8 °C Grade Count:12
Injection Pressure 3.50 - 120 MPaAverage value: 80.9 MPa Grade Count:45
Vent Depth 0.00127 - 0.00381 cmAverage value: 0.00154 cm Grade Count:7
Hot-Working Temperature 250 - 260 °CAverage value: 255 °C Grade Count:5
Precipitation Temperature 40.0 - 60.0 °CAverage value: 50.0 °C Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Polybutylene Terephthalate (PBT), 30% Glass Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), 10% Glass Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), Unreinforced, Molded
Overview of materials for Polybutylene Terephthalate (PBT), 40% Glass Fiber Filled
Overview of materials for Polybutylene Terephthalate (PBT), 50% Glass Fiber Filled

O3212 / 78172

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.