MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
BASF 3D Ultrafuse® PA6 GF30 30% Glass Fiber Reinforced, Fused Fillament, Dry
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled

Material Notes: Components: Polyamide based filament filled with 30% glass fibers for Fused Filament Fabrication.

Product Description: Ultrafuse® PA6 GF30 is polyamide, reinforced with 30% glass fiber content. The fibers in this material are specially designed for 3D-printing filaments and are compatible with a wide range of FFF 3D-printers. The extreme stiffness and strength make this material highly suitable for demanding applications. Ultrafuse® PA6 GF30 has a good chemical and wear resistance. With its excellent layer adhesion and the low warping, it is designed to be easy to use and suitable for a wide range of applications.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.519 g/ccPrinted Part; ISO 1183-1
Melt Flow 88.5577 g/10 min
@Load 5.00 kg,
Temperature 275 °C
ISO 1133
Storage Temperature 15.0 - 25.0 °C
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 14.9 MPaZX: Upright; ISO 527
 78.3 MPaXY: Flat; ISO 527
Elongation at Break 0.80 %ZX: Upright; ISO 527
 2.2 %XY: Flat; ISO 527
Modulus of Elasticity 2.38 GPaYoung's, ZX: Upright; ISO 527
 5.036 GPaYoung's, XY: Flat; ISO 527
Flexural Strength 44.2 MPaZX: Upright; ISO 178
 147.4 MPaXY: Flat; ISO 178
 188.2 MPaXZ: On its edge; ISO 178
Flexural Modulus 2371 MPaZX: Upright; ISO 178
 4694 MPaXY: Flat; ISO 178
 8103 MPaXZ: On its edge; ISO 178
Flexural Strain at Break 2.0 %ZX: Upright; ISO 178
 2.7 %XZ: On its edge; ISO 178
 4.0 %XY: Flat; ISO 178
Izod Impact, Notched (ISO) 9.20 kJ/m²XY: Flat; ISO 180
 13.4 kJ/m²XZ: On its edge; ISO 180
Izod Impact, Unnotched (ISO) 2.60 kJ/m²ZX: Upright; ISO 180
 38.4 kJ/m²XY: Flat; ISO 180
 38.7 kJ/m²XZ: On its edge; ISO 180
Charpy Impact Unnotched 2.20 kJ/m²ZX: Upright; ISO 179
 38.9 kJ/m²XY: Flat; ISO 179
 45.5 kJ/m²XZ: On its edge; ISO 179
Charpy Impact, Notched 8.90 kJ/m²XY: Flat; ISO 179
 16.2 kJ/m²XZ: On its edge; ISO 179
 
Thermal PropertiesOriginal ValueComments
Melting Point 209 °CISO 11357-3
Crystallization Temperature 167 °CISO 11357-3
Deflection Temperature at 0.46 MPa (66 psi) 110 °CISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 82.0 °CISO 75-2
Vicat Softening Point 192 °C
@Load 5.10 kg
ISO 306
Glass Transition Temp, Tg 67.0 °CISO 11357-2
 
Processing PropertiesOriginal ValueComments
Processing Temperature 70.0 - 100 °CBed, Bed Material: Glass
Nozzle Temperature 240 - 280 °C
Drying Temperature 100 °Cin a hot air dryer or vacuum oven
Dry Time 4.00 - 16.0 hour
Shelf Life 12.0 Month
 
Descriptive Properties
Nozzle Diameter=0.6 mm
Print speed30-60 mm/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PBASF3D017 / 312258

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.