MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sumitomo Bakelite North America Epiall® 1904B-1 Short Glass Fiber Reinforced Epoxy
Categories: Polymer; Thermoset; Epoxy; Epoxy, Molded, Glass Fiber Filler; Filled/Reinforced Thermoset

Material Notes: Epiall 1904B-1 is a short fiberglass reinforced epoxy molding compound, with excellent dimensional stability, good strength properties and good electrical insulation properties.

Information provided by Sumitomo Bakelite North America, Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.900 g/ccASTM D1895
Density 2.09 g/ccASTM D792
Water Absorption 0.20 %
@Temperature 50.0 °C,
Time 173000 sec
ASTM D570
Linear Mold Shrinkage 0.0010 - 0.0030 cm/cmASTM D955
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 90.0 MPaASTM D638
Flexural Strength 140 MPaat rupture; ASTM D790
Flexural Modulus 23.0 GPaASTM D790
Compressive Strength 210 MPaASTM D695
Izod Impact, Notched 33.0 J/mASTM D256
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 4.6
@Frequency 1e+6 Hz
wet; ASTM D150
Dielectric Strength 13.8 kV/mm
@Frequency 60 Hz
step-by-step, wet; ASTM D149
 14.5 kV/mm
@Frequency 60 Hz
short time, wet; ASTM D149
Dissipation Factor 0.035
@Frequency 1e+6 Hz
wet; ASTM D150
Arc Resistance 189 secASTM D495
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) 280 °CAs Molded; ASTM D648A
 >= 282 °CPost Baked; ASTM D648A
 
Descriptive Properties
ColorsBlack, Green
FormGranular
Molding MethodCompression
 Transfer

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Sumitomo Bakelite North America Epiall® 1914A Short Glass Fiber Reinforced Epoxy
Sumitomo Bakelite North America Epiall® 1908B-1 Short Glass Fiber Reinforced Epoxy
Sumitomo Bakelite North America Epiall® 1908M-1 Short Glass Fiber Reinforced Epoxy
Sumitomo Bakelite North America Epiall® 1908-1 Short Glass Fiber Reinforced Epoxy
Overview of materials for Epoxy, Molded, Glass Fiber Filler

P90X917 / 142692

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.