MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
SABIC LNP™ LUBRILOY™ Compound RF203 Polyamide 66 (Nylon 66)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: LNP LUBRILOY RF203 compound is based on Nylon 6/6 resin containing 15% glass fiber and proprietary lubricant. Added features of this grade include: Internally Lubricated, Wear Resistant.

Features: Internally Lubricated,Wear resistant

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.12 g/ccISO 1183
Water Absorption 0.37 %
@Time 86400 sec
ISO 62-1
Moisture Absorption 0.150 - 0.250 %Injection Molding
Linear Mold Shrinkage, Flow 0.0030 - 0.0050 cm/cmSABIC method
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 99.0 MPa5 mm/min; ISO 527
Elongation at Break 3.5 %5 mm/min; ISO 527
Tensile Modulus 5300 MPa1 mm/min; ISO 527
Flexural Strength 122 MPabreak, 2mm/min; ISO 178
 133 MPayield, 2 mm/min; ISO 178
Flexural Modulus 4100 MPa2 mm/min; ISO 178
Izod Impact, Notched (ISO) 9.00 kJ/m²80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 50.0 kJ/m²80*10*4; ISO 180/1U
Coefficient of Friction, Dynamic 0.36ASTM D3702 Modified: Manual
Coefficient of Friction, Static 0.30ASTM D3702 Modified: Manual
K (wear) Factor 70.0 x 10-10 in³-min/ft-lb-hrWasher; ASTM D3702 Modified: Manual
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 41.0 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 131 µm/m-°C
@Temperature 23.0 - 60.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 245 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
Deflection Temperature at 1.8 MPa (264 psi) 185 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
UL RTI, Electrical 65.0 °CUL 746B
UL RTI, Mechanical with Impact 65.0 °CUL 746B
UL RTI, Mechanical without Impact 65.0 °CUL 746B
Flammability, UL94 HB
@Thickness 1.50 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Zone 2 280 - 295 °C
Zone 3 295 - 305 °C
Melt Temperature 270 - 280 °CInjection Molding
Mold Temperature 80.0 - 95.0 °C
Drying Temperature 80.0 °CInjection Molding
Dry Time 4.00 hourInjection Molding
Back Pressure 0.200 - 0.300 MPa
Screw Speed 30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH81146 / 289093

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.