MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
Carmel Olefins Ipethene® 4203 LDPE Film Grade
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); Low Density (LDPE); Low Density Polyethylene (LDPE), Film Grade

Material Notes: IPETHENE® 4203 is a low-density polyethylene film grade, produced by high-pressure autoclave technology. Features: No additives, Good environmental stress, cracking resistance, Excellent bubble stability, Good mechanical properties. Uses: Large diameter agricultural films, Construction films, Shrink films, Pipes, Heavy duty bags. Processing Methods: Blown film extrusion, Blow molding, Pipe extrusion.

Property data measured on samples of 100 µm blown film, Blow-up ratio 2.5:1, output 10 kg/h, melt temperature ~210°C.

Information provided by Carmel Olefins Ltd.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.920 g/ccISO 1183-A
Thickness 100 micronsAs Tested
Melt Flow 0.20 g/10 min
@Load 2.16 kg,
Temperature 190 °C
1133
 
Mechanical PropertiesOriginal ValueComments
Film Elongation at Break, MD 650 %
@Thickness 0.100 mm
blown film; ISO 527-3
Film Elongation at Break, TD 700 %
@Thickness 0.100 mm
blown film; ISO 527-3
Elmendorf Tear Strength MD 250 g
@Thickness 0.100 mm
blown film; ISO 6383-2
Elmendorf Tear Strength TD 450 g
@Thickness 0.100 mm
blown film; ISO 6383-2
Dart Drop Test 500 g
@Thickness 0.100 mm
F50. blown film; ISO 7765-A
Film Tensile Strength at Break, MD 23.0 MPa
@Thickness 0.100 mm
blown film; ISO 527-3
Film Tensile Strength at Break, TD 26.0 MPa
@Thickness 0.100 mm
blown film; ISO 527-3
 
Thermal PropertiesOriginal ValueComments
Melting Point 109 °CBy DSC; ISO 11357-3
Vicat Softening Point 97.0 °C
@Load 1.02 kg
ISO 306
 
Processing PropertiesOriginal ValueComments
Melt Temperature 210 °CAs Tested

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PCARM826 / 249046

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.