MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SABIC LEXAN™ Copolymer EXL9414P Polycarbonate (PC)
Categories: Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: LEXAN EXL9414P polycarbonate (PC) siloxane copolymer resin is a medium flow, non-chlorinated, non-brominated flame retardant opaque injection molding (IM) grade. This resin offers low temperature ductility, thin wall flame retardant capability, and in combination with excellent processability and release with opportunities for shorter IM cycle times compared to standard PC. LEXAN EXL9414P copolymer resin is a product available in wide range of opaque colors and may be an excellent candidate for a wide variety of applications, especially the housing of fast-charging mobile phones.

Features: Enhanced Low Temperature Impact,Flame Retardant,Non-Chlorinated,Non-Brominated,High Impact Resistance,Good Processability

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.19 g/ccASTM D792
Density 1.19 g/ccISO 1183
Moisture Absorption 0.0200 %Injection Molding
Viscosity 12 cP
@Load 1.20 kg,
Temperature 300 °C
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0040 - 0.0080 cm/cmSABIC method
Linear Mold Shrinkage, Transverse 0.0040 - 0.0080 cm/cmSABIC method
Melt Flow 13.5 g/10 min
@Load 1.20 kg,
Temperature 300 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 55.0 MPa50 mm/min; ASTM D638
 56.0 MPa50 mm/min; ISO 527
Elongation at Break 63 %50 mm/min; ISO 527
 89 %50 mm/min; ASTM D638
Elongation at Yield 4.9 %50 mm/min; ISO 527
 5.3 %50 mm/min; ASTM D638
Tensile Modulus 2109 MPa1 mm/min; ISO 527
 2117 MPa50 mm/min; ASTM D638
Flexural Strength 86.0 MPayield, 2 mm/min; ISO 178
 90.0 MPayld, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2184 MPa2 mm/min; ISO 178
 2200 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact Notched 962 JASTM D256
 670 J
@Temperature -30.0 °C
ASTM D256
Izod Impact, Notched (ISO) 77.0 kJ/m²80*10*3; ISO 180/1A
 51.0 kJ/m²
@Temperature -30.0 °C
80*10*3; ISO 180/1A
Charpy Impact, Notched 81.0 kJ/m²Edgew 80*10*3 sp=62mm; ISO 179/1eA
 48.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*3 sp=62mm; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 2.82
@Frequency 1.90e+9 Hz
SABIC method
 2.82
@Frequency 5.00e+9 Hz
SABIC method
 2.83
@Frequency 1e+10 Hz
SABIC method
 2.87
@Frequency 1.10e+9 Hz
SABIC method
Dissipation Factor 0.0060
@Frequency 1.10e+9 Hz
SABIC method
 0.0060
@Frequency 1.90e+9 Hz
SABIC method
 0.0060
@Frequency 5.00e+9 Hz
SABIC method
 0.0060
@Frequency 1e+10 Hz
SABIC method
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 77.1 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 91.1 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 83.4 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 95.4 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 124 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 123 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 111 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 110 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 137 °CRate B/50; ISO 306
 138 °CRate B/120; ISO 306
UL RTI, Electrical 80.0 °CUL 746B
UL RTI, Mechanical with Impact 80.0 °CUL 746B
UL RTI, Mechanical without Impact 80.0 °CUL 746B
Flammability, UL94 V-0
@Thickness 0.800 mm
UL 94
Glow Wire Ignition Temperature 825 °C
@Thickness 1.00 mm
IEC 60695-2-13
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 290 - 310 °C
Zone 2 280 - 305 °C
Zone 3 295 - 315 °C
Melt Temperature 295 - 315 °CInjection Molding
Mold Temperature 70.0 - 95.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 48.0 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 60 %
Vent Depth 0.00250 - 0.00760 cm
Screw Speed 40 - 70 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABH80242 / 288189

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.