MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
SABIC VALOX™ 420HP PBT (Americas)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: 30% Glass filled PBT resin, FDA Food Contact compliant in limited colors. Effective March 2008 this grade will no longer be supported with biocompatibility information. Alternative grade VALOX HX420HP.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.53 g/ccASTM D792
 1.53 g/ccASTM D792
Density 1.53 g/ccISO 1183
Filler Content 30 %ASTM D229
Water Absorption 0.060 %24 hours; ASTM D570
 0.26 %23°C/sat; ISO 62
Moisture Absorption 0.0800 %23°C / 50% RH; ISO 62
Linear Mold Shrinkage, Flow 0.0030 - 0.0070 cm/cmSABIC method
 0.0030 - 0.0050 cm/cm
@Thickness 1.50 - 3.20 mm
SABIC method
 0.0030 - 0.0080 cm/cm
@Thickness 3.20 mm
SABIC method
 0.0050 - 0.0080 cm/cm
@Thickness 3.20 - 4.60 mm
SABIC method
Linear Mold Shrinkage, Transverse 0.0050 - 0.010 cm/cmSABIC method
 0.0040 - 0.0060 cm/cm
@Thickness 1.50 - 3.20 mm
SABIC method
 0.0060 - 0.0090 cm/cm
@Thickness 3.20 - 4.60 mm
SABIC method
 0.0050 - 0.010 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 13 g/10 min
@Load 2.16 kg,
Temperature 250 °C
cm³/10 min; ISO 1133
 17 g/10 min
@Load 2.16 kg,
Temperature 250 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 118ASTM D785
Tensile Strength at Break 120 MPa5 mm/min; ASTM D638
 125 MPa5 mm/min; ISO 527
Tensile Strength, Yield 120 MPa5 mm/min; ASTM D638
 125 MPa5 mm/min; ISO 527
Elongation at Break 2.0 %5 mm/min; ISO 527
 3.0 %5 mm/min; ASTM D638
Elongation at Yield 2.0 %5 mm/min; ISO 527
 3.0 %5 mm/min; ASTM D638
Tensile Modulus 9300 MPa1mm/min; ISO 527
 9300 MPa5 mm/min; ASTM D638
Flexural Strength 189 MPabrk, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Yield Strength 195 MPa2 mm/min; ISO 178
Flexural Modulus 7580 MPa1.3 mm/min, 50 mm span; ASTM D790
 8500 MPa2 mm/min; ISO 178
Izod Impact, Notched 85.0 J/mASTM D256
 80.0 J/m
@Temperature -30.0 °C
ASTM D256
Izod Impact, Unnotched 801 J/mASTM D4812
Izod Impact, Notched (ISO) 8.00 kJ/m²80*10*4; ISO 180/1A
 7.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 45.0 kJ/m²80*10*4; ISO 180/1U
 45.0 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched 45.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eU
 45.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 5.00 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 5.00 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 8.00 JASTM D3763
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 3.20e+16 ohm-cmASTM D257
Dielectric Constant 3.7
@Frequency 1e+6 Hz
ASTM D150
 3.8
@Frequency 100 Hz
ASTM D150
Dielectric Strength 18.7 kV/mm
@Thickness 3.20 mm
in air; ASTM D149
 24.8 kV/mm
@Thickness 1.60 mm
in oil; ASTM D149
Dissipation Factor 0.0020
@Frequency 100 Hz
ASTM D150
 0.020
@Frequency 1e+6 Hz
ASTM D150
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 25.2 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 25.2 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
CTE, linear, Transverse to Flow 120 µm/m-°C
@Temperature -40.0 - 40.0 °C
ASTM E831
 120 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 217 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 215 °C
@Thickness 6.40 mm
unannealed; ASTM D648
 220 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 204 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 203 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 215 °CRate B/50; ASTM D1525
 215 °CRate B/50; ISO 306
 215 °CRate B/120; ISO 306
 223 °CRate A/50; ISO 306
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 245 - 260 °CInjection Molding
Zone 1 240 - 255 °C
Zone 2 245 - 260 °C
Zone 3 250 - 265 °C
Melt Temperature 250 - 265 °C
Mold Temperature 65.0 - 90.0 °C
Drying Temperature 120 °CInjection Molding
Dry Time 3.00 - 4.00 hourInjection Molding
 12.0 hourCumulative; Injection Molding
Moisture Content 0.020 %
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 80 %
Vent Depth 0.00250 - 0.00380 cm
Screw Speed 50 - 80 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10257 / 243724

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.