MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Delrin Delrin® SC655 NC010 POM
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: Medium Viscosity Acetal Homopolymer Developed for the Healthcare Industry

Information provided by DuPont; Delrin was sold by DuPont in 2023.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.42 g/ccISO 1183
Water Absorption 1.4 %
@Thickness 2.00 mm
Sim. to ISO 62
Moisture Absorption 0.300 %
@Thickness 2.00 mm
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.020 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.019 cm/cmISO 294-4, 2577
Melt Flow 15 g/10 minISO 1133
 13 g/10 min
@Load 2.16 kg,
Temperature 190 °C
cm³/10min Volumetric; ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Puncture Resistance 2000 N
@Temperature 23.0 °C
maximum force; ISO 6603-2
Hardness, Rockwell M 92ISO 2039-2
Hardness, Rockwell R 120ISO 2039-2
Tensile Strength, Yield 71.0 MPaISO 527-1/-2
Elongation at Break 30 %Nominal; ISO 527-1/-2
Elongation at Yield 17 %ISO 527-1/-2
Tensile Modulus 3100 MPaISO 527-1/-2
Flexural Strength 80.0 MPa
@Strain 3.5 %
ISO 178
Flexural Modulus 2950 MPaISO 178
Poissons Ratio 0.37
Izod Impact, Notched (ISO) 8.00 kJ/m²
@Temperature -30.0 °C
ISO 180/1A
 9.00 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
Izod Impact, Unnotched (ISO) 250 kJ/m²
@Temperature -30.0 °C
ISO 180/1U
 280 kJ/m²
@Temperature 23.0 °C
ISO 180/1U
Charpy Impact Unnotched 280 kJ/m²
@Temperature -30.0 °C
ISO 179/1eU
 300 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 8.00 kJ/m²
@Temperature -30.0 °C
ISO 179/1eA
 9.00 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
Puncture Energy 3.00 J
@Temperature 23.0 °C
ISO 6603-2
Tensile Creep Modulus, 1 hour 2800 MPa1h; ISO 899-1
Tensile Creep Modulus, 1000 hours 1600 MPa1000h; ISO 899-1
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 2.00e+14 ohm-cmIEC 62631-3-1
Surface Resistance 4.00e+14 ohmIEC 62631-3-2
Dielectric Constant 3.8
@Frequency 1e+6 Hz
IEC 62631-2-1
 3.8
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 44.0 kV/mmIEC 60243-1
Dissipation Factor 0.0055
@Frequency 1e+6 Hz
IEC 62631-2-1
 0.0090
@Frequency 100 Hz
IEC 62631-2-1
Comparative Tracking Index 600 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 110 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 110 µm/m-°CISO 11359-1/-2
Melting Point 178 °C10°C/min; ISO 11357-1/-3
Hot Ball Pressure Test 165 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 160 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 95.0 °CISO 75-1/-2
Vicat Softening Point 155 °C50°C/h, 50N; ISO 306
 
Processing PropertiesOriginal ValueComments
Melt Temperature 215 °COptimum, Injection
 210 - 220 °CRange, Injection
Mold Temperature 90.0 °COptimum, Injection
 80.0 - 100 °CInjection
Drying Temperature 80.0 °CInjection
Dry Time 2.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.20 %Injection
Hold Pressure 80.0 - 100 MPaInjection
 100 MPaInjection
Annealing Temperature 160 °COptional; 2 mm/min; Injection
 
Descriptive Properties
AdditivesRelease agent
Annealing time (min/mm)30Optional, Injection
Drying RecommendedyesInjection
Emissions (mg/kg)<8VDA 275
Fogging (%)90F-value (refraction); ISO 6452
Fogging (mg)0.35G-value (condensate); ISO 6452
Part Marking Code>POM<ISO 11469
PolymerPOM
Processing Hold Pressure Time (s/mm)8Injection
Resin IdentificationPOMISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Delrin® SC699 NC010 POM
INEOS Styrolution Novodur® M203FC ABS
Colorite Polymers 1124 Clear Injection Molding Vinyl Compound
INEOS Styrolution Terlux® 2802 Transparent MABS
Delrin Delrin® 500CL BK601 POM

PDSX5163 / 197803

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.