MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Sandvik SANMAC 304/304L Hollow Bar
Categories: Metal; Ferrous Metal; Austenitic; Stainless Steel; T 300 Series Stainless Steel

Material Notes: Sandvik SANMAC 304L is an austenitic chromium-nickel steel with improved machinability.

Information provided by Sandvik

ASTM 304, 304L; UNS S30400, S30403; EN 1.4301, 1.4307

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 7.90 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B <= 90
Tensile Strength, Ultimate >= 305 MPa
@Temperature 600 °C
 >= 325 MPa
@Temperature 550 °C
 >= 345 MPa
@Temperature 500 °C
 >= 355 MPa
@Temperature 450 °C
 >= 365 MPa
@Temperature 400 °C
 >= 370 psi
@Temperature 350 °C
 >= 380 MPa
@Temperature 300 °C
 >= 390 MPa
@Temperature 250 °C
 >= 400 MPa
@Temperature 200 °C
 >= 425 MPa
@Temperature 150 °C
 >= 450 MPa
@Temperature 100 °C
 >= 480 MPa
@Temperature 50.0 °C
 515 - 680 MPa
@Thickness 10.0 mm
wall thickness
Tensile Strength, Yield >= 210 MPa
@Strain 0.2 %
10 mm wall thickness
 >= 240 MPa
@Strain 1 %
10 mm wall thickness
 >= 95.0 MPa
@Strain 0.2 %,
Temperature 600 °C
 >= 100 MPa
@Strain 0.2 %,
Temperature 550 °C
 >= 105 MPa
@Strain 0.2 %,
Temperature 500 °C
 >= 110 MPa
@Strain 0.2 %,
Temperature 450 °C
 >= 115 MPa
@Strain 0.2 %,
Temperature 400 °C
 >= 120 MPa
@Strain 0.2 %,
Temperature 350 °C
 >= 120 ksi
@Strain 1 %,
Temperature 600 °C
 >= 125 MPa
@Strain 1 %,
Temperature 550 °C
 >= 125 MPa
@Strain 0.2 %,
Temperature 300 °C
 >= 130 MPa
@Strain 1 %,
Temperature 500 °C
 >= 130 MPa
@Strain 0.2 %,
Temperature 250 °C
 >= 135 MPa
@Strain 1 %,
Temperature 450 °C
 >= 140 MPa
@Strain 1 %,
Temperature 400 °C
 >= 140 MPa
@Strain 0.2 %,
Temperature 200 °C
 >= 145 MPa
@Strain 1 %,
Temperature 350 °C
 >= 150 MPa
@Strain 0.2 %,
Temperature 150 °C
 >= 150 MPa
@Strain 1 %,
Temperature 300 °C
 >= 155 MPa
@Strain 1 %,
Temperature 250 °C
 >= 165 MPa
@Strain 1 %,
Temperature 200 °C
 >= 165 MPa
@Strain 0.2 %,
Temperature 100 °C
 >= 175 MPa
@Strain 1 %,
Temperature 150 °C
 >= 190 MPa
@Strain 0.2 %,
Temperature 50.0 °C
 >= 195 MPa
@Strain 1 %,
Temperature 100 °C
 >= 215 MPa
@Strain 1 %,
Temperature 50.0 °C
Elongation at Break >= 35 %2", 10 mm wall thickness
 >= 45 %
@Thickness 10.0 mm
wall thickness
Modulus of Elasticity 200 GPa
 165 GPa
@Temperature 500 °C
 172 GPa
@Temperature 400 °C
 179 GPa
@Temperature 300 °C
 186 GPa
@Temperature 200 °C
 194 GPa
@Temperature 100 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 16.5 µm/m-°C
@Temperature 30.0 - 100 °C
 17.0 µm/m-°C
@Temperature 30.0 - 200 °C
 17.5 µm/m-°C
@Temperature 30.0 - 300 °C
 18.0 µm/m-°C
@Temperature 30.0 - 400 °C
 18.5 µm/m-°C
@Temperature 30.0 - 600 °C
 18.5 µm/m-°C
@Temperature 30.0 - 500 °C
 19.0 µm/m-°C
@Temperature 30.0 - 700 °C
Specific Heat Capacity 0.475 J/g-°C
@Temperature 20.0 °C
 0.500 J/g-°C
@Temperature 100 °C
 0.530 J/g-°C
@Temperature 200 °C
 0.560 J/g-°C
@Temperature 300 °C
 0.580 J/g-°C
@Temperature 400 °C
 0.600 J/g-°C
@Temperature 500 °C
 0.615 J/g-°C
@Temperature 600 °C
 0.625 J/g-°C
@Temperature 700 °C
Thermal Conductivity 15.0 W/m-K
@Temperature 20.0 °C
 16.0 W/m-K
@Temperature 100 °C
 18.0 W/m-K
@Temperature 200 °C
 20.0 W/m-K
@Temperature 300 °C
 22.0 W/m-K
@Temperature 400 °C
 23.0 W/m-K
@Temperature 500 °C
 25.0 W/m-K
@Temperature 600 °C
 26.0 W/m-K
@Temperature 700 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.030 %
Chromium, Cr 18.5 %
Iron, Fe 70.7 %As Balance
Manganese, Mn 1.3 %
Nickel, Ni 9.0 %
Phosphorus, P <= 0.040 %
Silicon, Si 0.40 %
Sulfur, S <= 0.030 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304L, 0% Cold Rolled (UNS S30403)
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304L, Annealed (UNS S30403)
Eagle Brass 304L Austenitic Stainless Steel, Annealed
Ametek Ultra 304L P/M Stainless Steel, Sintered from 6.2 g/cc Green Density
AISI Type 316L Stainless Steel, annealed sheet

NSANDV188 / 19082

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.