MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
ATI Allegheny Ludlum 410 Martensitic Stainless Steel
Categories: Metal; Ferrous Metal; Martensitic; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Characteristics: superior wear resistance, hardenable, excellent corrosion resistance.

Applications:cutlery, dental and surgical instruments, nozzles, valve parts, hardened steel ball and seats for oil well pumps, separating screens and strainers, springs, shears, and wear surfaces.

Information provided by Allegheny Ludlum

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Specific Gravity 7.65 g/cc
Density 7.64 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell B 82
 98Hardened+Tempered 1200°F
Hardness, Rockwell C 35Hardened+Tempered 1000°F
 40Hardened+Tempered 550°F
 40Hardened+Tempered 600°F
 41Hardened+Tempered 800°F
 41Hardened+Tempered 900°F
 43Hardened+Tempered 400°F
Tensile Strength, Ultimate 510 MPaAnnealed
 767 MPaHardened 1800°F, Tempered 1200°F
 1063 MPaHardened 1800°F, Tempered 1000°F
 1283 MPaHardened 1800°F, Tempered 600°F
 1289 MPaHardened 1800°F, Tempered 550°F
 1298 MPaHardened 1800°F, Tempered 900°F
 1300 MPaHardened 1800°F, Tempered 800°F
 1399 MPaHardened 1800°F, Tempered 400°F
Tensile Strength, Yield 589 MPaHardened 1800°F, Tempered 1200°F
 845 MPaHardened 1800°F, Tempered 900°F
 882 MPaHardened 1800°F, Tempered 1000°F
 916 MPaHardened 1800°F, Tempered 800°F
 1022 MPaHardened 1800°F, Tempered 550°F
 1026 MPaHardened 1800°F, Tempered 600°F
 1076 MPaHardened 1800°F, Tempered 400°F
 290 MPa
@Strain 0.2 %
Annealed
Elongation at Break 34 %Annealed
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000560 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.5 µm/m-°C
@Temperature 20.0 - 200 °C
 11.6 µm/m-°C
@Temperature 20.0 - 600 °C
Specific Heat Capacity 0.460 J/g-°C
Thermal Conductivity 24.9 W/m-K
@Temperature 100 °C
Melting Point 1482 - 1532 °C
Solidus 1482 °C
Liquidus 1532 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.15 %
Chromium, Cr 11.5 - 13.5 %
Iron, Fe 83.8 - 88.5 %as balance
Manganese, Mn <= 1.0 %
Nickel, Ni <= 0.50 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.030 %
 
Descriptive Properties
Corrosion Rate mils per year0.062 (5% Phosphoric Acid at 49°C)Hardened martensitic grades were tested after tempering at 204°C
 0.079 (5% Acetic Acid at 49°C)Hardened martensitic grades were tested after tempering at 204°C.
Pitting Potential, Volts vs. Sat. Calomel Electrode0.502100 ppm Chloride solution at 24°C, pH5, ground surface. Hardened martensitic grades were tested after tempering at 204°C.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
410 Stainless Steel
304 Stainless Steel
ATI Allegheny Ludlum Stainless Steel Chromium-Nickel Type 304, Annealed (UNS S30400)
410 Stainless Steel, tempered at 343°C
410 Stainless Steel, tempered at 453°C

NL1034 / 17802

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.