MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Henkel Loctite® Stycast® US 5529 Two-Component Flexible, Flame Retardant, Polyurethane Compound
Categories: Polymer; Thermoset; Polyurethane, TS

Material Notes: Loctite Stycast US 5529 provides the following product characteristics: Room temperature cure

Application: Potting and Encapsulating

Loctite Stycast US 5529 is a flexible, flame retardant, mineral filled, polyurethane compound. This potting compound has long pot life, and is low viscosity so it flows well and adheres well to many substrates. It has very low odor and does not contain TDI or mercury compounds. Although Loctite Stycast US 5529 is not UL recognized, it does have the same amount of flame retardant chemical as US5528, which is UL recognized.

Information provided by Henkel.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.50 g/ccCured
Moisture Absorption 0.0100 %
@Time 86400 sec
Viscosity 2400 cPMixed
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 85
Tensile Strength 540 psi
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 4.50e+13 ohm-cm
Dielectric Constant 4.0
@Frequency 100000 Hz
Dielectric Strength 972 V/mil
Dissipation Factor 0.040
@Frequency 100000 Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear 150 µm/m-°C
Thermal Conductivity 0.335 W/m-K
Flammability, UL94 V-0
@Thickness 6.10 mm
 V-0
@Thickness 9.53 mm
 
Processing PropertiesOriginal ValueComments
Cure Time 1.00 - 3.00 hour
@Temperature 65.0 - 85.0 °C
Alternate
 12.0 - 24.0 hour
@Temperature 22.0 - 30.0 °C
Recommended
Working Life >= 45.0 min
@Temperature 23.0 °C
300 gm mass
Gel Time 90.0 min300 gm mass
 
Descriptive Properties
AppearanceBlackCured
Mix Ratio, by Volume1 : 4.81Part A : Part B
Mix Ratio, by Weight15 : 85Component A : Component B
Weight Loss (%)0.004Weight Loss after 168 hrs @ 130ºC

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PHENK7969 / 255453

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.