MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
DuPont Mobility and Materials Zytel® HTN 52G35HSL NC010 Polyphthalamide (PPA) (Extended Tabular Temperature Data)  (discontinued **)
Categories: Polymer; Thermoplastic; Polyphthalamide (PPA); Polyphthalamide (PPA), 40% Glass Fiber Reinforced

Material Notes: Zytel® HTN52G35HSL NC010 is a 35% glass reinforced, heat stabilized, lubricated high performance polyamide resin that can be molded in water heated molds.

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.47 g/ccDAM; ASTM D792
Density 1.45 g/ccDAM; ISO 1183
Filler Content 35 %DAM
Linear Mold Shrinkage 0.010 cm/cm
@Thickness 1.60 mm
Transverse; DAM
 0.010 cm/cm
@Thickness 3.20 mm
Transverse; DAM
Linear Mold Shrinkage, Flow 0.0020 cm/cm
@Thickness 2.00 mm
DAM; ISO 294-4
 0.0025 cm/cm
@Thickness 1.60 mm
Flow; DAM
 0.0030 cm/cm
@Thickness 3.20 mm
Flow; DAM
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 105DAM; ASTM D785
Hardness, Rockwell R 124DAM; ASTM D785
Tensile Strength at Break 180 MPa
@Temperature 23.0 °C
50%RH; ISO 527
 200 MPa
@Temperature 23.0 °C
DAM; ISO 527
Tensile Strength 72.4 MPa
@Temperature 200 °C
DAM; ASTM D638
 80.0 MPa
@Temperature 175 °C
DAM; ASTM D638
 89.0 MPa
@Temperature 150 °C
DAM; ASTM D638
 124 MPa
@Temperature 100 °C
DAM; ASTM D638
 168 MPa
@Temperature 23.0 °C
50%RH; ASTM D638
 188 MPa
@Temperature 60.0 °C
DAM; ASTM D638
 204 MPa
@Temperature 23.0 °C
DAM; ASTM D638
 230 MPa
@Temperature -40.0 °C
DAM; ASTM D638
Elongation at Break 2.1 %
@Temperature 23.0 °C
DAM; ISO 527
 2.3 %
@Temperature -40.0 °C
DAM; ASTM D638
 2.3 %
@Temperature 23.0 °C
DAM; ASTM D638
 2.7 %
@Temperature 23.0 °C
50%RH; ISO 527
 2.8 %
@Temperature 60.0 °C
DAM; ASTM D638
 3.3 %
@Temperature 23.0 °C
50%RH; ASTM D638
 4.5 %
@Temperature 100 °C
DAM; ASTM D638
 5.4 %
@Temperature 200 °C
DAM; ASTM D638
 5.5 %
@Temperature 150 °C
DAM; ASTM D638
 5.5 %
@Temperature 175 °C
DAM; ASTM D638
Tensile Modulus 4400 MPa
@Temperature 200 °C
DAM; ASTM D638
 4800 MPa
@Temperature 175 °C
DAM; ASTM D638
 5200 MPa
@Temperature 150 °C
DAM; ASTM D638
 7300 MPa
@Temperature 100 °C
DAM; ASTM D638
 10300 MPa
@Temperature 23.0 °C
50%RH; ASTM D638
 11200 MPa
@Temperature 60.0 °C
DAM; ASTM D638
 11700 MPa
@Temperature -40.0 °C
DAM; ASTM D638
 11700 MPa
@Temperature 23.0 °C
DAM; ASTM D638
 12000 MPa
@Temperature 23.0 °C
50%RH; ISO 527
 12500 MPa
@Temperature 23.0 °C
DAM; ISO 527
Flexural Strength 249 MPa
@Temperature 23.0 °C
50%RH; ASTM D790
 261 MPa
@Temperature 60.0 °C
DAM; ASTM D790
 299 MPa
@Temperature 23.0 °C
DAM; ASTM D790
 352 MPa
@Temperature -40.0 °C
DAM; ASTM D790
 96.0 MPa
@Strain 5.0 %,
Temperature 200 °C
DAM; ASTM D790
 114 MPa
@Strain 5.0 %,
Temperature 175 °C
DAM; ASTM D790
 128 MPa
@Strain 5.0 %,
Temperature 150 °C
DAM; ASTM D790
 181 MPa
@Strain 5.0 %,
Temperature 100 °C
DAM; ASTM D790
Flexural Modulus 3460 MPa
@Temperature 200 °C
DAM; ASTM D790
 3630 MPa
@Temperature 175 °C
DAM; ASTM D790
 3810 MPa
@Temperature 150 °C
DAM; ASTM D790
 5090 MPa
@Temperature 100 °C
DAM; ASTM D790
 8300 MPa
@Temperature 23.0 °C
50%RH; ASTM D790
 9190 MPa
@Temperature 60.0 °C
DAM; ASTM D790
 10190 MPa
@Temperature 23.0 °C
DAM; ASTM D790
 10620 MPa
@Temperature -40.0 °C
DAM; ASTM D790
Compressive Strength 71.0 MPa
@Temperature 200 °C
DAM; ASTM D695
 89.0 MPa
@Temperature 175 °C
DAM; ASTM D695
 102 MPa
@Temperature 150 °C
DAM; ASTM D695
 166 MPa
@Temperature 100 °C
DAM; ASTM D695
 245 MPa
@Temperature 60.0 °C
DAM; ASTM D695
 281 MPa
@Temperature 23.0 °C
DAM; ASTM D695
 355 MPa
@Temperature -40.0 °C
DAM; ASTM D695
Shear Strength 79.3 MPa
@Temperature 23.0 °C
50%RH; ASTM D732
 91.7 MPa
@Temperature 23.0 °C
DAM; ASTM D732
Izod Impact, Notched 91.0 J/m
@Temperature -40.0 °C
50%RH; ASTM D256
 91.0 J/m
@Temperature -40.0 °C
DAM; ASTM D256
 91.0 J/m
@Temperature 23.0 °C
DAM; ASTM D256
 91.0 J/m
@Temperature 23.0 °C
50%RH; ASTM D256
Izod Impact, Unnotched 8.50 J/cm
@Temperature 23.0 °C
50%RH; ASTM D4812
 10.1 J/cm
@Temperature 23.0 °C
DAM; ASTM D4812
Izod Impact, Unnotched (ISO) 40.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 180/1U
 45.0 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 180/1U
Charpy Impact Unnotched 35.0 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eU
 40.0 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eU
 40.0 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 179/1eU
 45.0 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eU
Charpy Impact, Notched 6.00 kJ/m²
@Temperature -30.0 °C
50%RH; ISO 179/1eA
 7.00 kJ/m²
@Temperature -30.0 °C
DAM; ISO 179/1eA
 9.00 kJ/m²
@Temperature 23.0 °C
DAM; ISO 179/1eA
 9.50 kJ/m²
@Temperature 23.0 °C
50%RH; ISO 179/1eA
Tensile Creep Modulus, 1 hour 10000 MPa
@Temperature 23.0 °C
50%RH; ISO 899
Tensile Creep Modulus, 1000 hours 8500 MPa
@Temperature 23.0 °C
50%RH; ISO 899
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cm
@Temperature 23.0 °C
DAM; ASTM D257
 1.00e+15 ohm-cm
@Temperature 23.0 °C
DAM; IEC 60093
Surface Resistance 1.00e+15 ohm
@Temperature 23.0 °C
DAM; ASTM D257
 1.00e+15 ohm
@Temperature 23.0 °C
50%RH; IEC 60093
Dielectric Constant 3.8
@Frequency 1e+6 Hz,
Temperature 23.0 °C
DAM; ASTM D150
 3.9
@Frequency 1000 Hz,
Temperature 23.0 °C
DAM; ASTM D150
 4.2
@Frequency 1e+6 Hz,
Temperature 60.0 °C
DAM; ASTM D150
 4.4
@Frequency 1000 Hz,
Temperature 60.0 °C
DAM; ASTM D150
 4.7
@Frequency 1e+6 Hz,
Temperature 100 °C
DAM; ASTM D150
 5.6
@Frequency 1000 Hz,
Temperature 100 °C
DAM; ASTM D150
 7.9
@Frequency 1e+6 Hz,
Temperature 150 °C
DAM; ASTM D150
 9.9
@Frequency 1e+6 Hz,
Temperature 175 °C
DAM; ASTM D150
 12
@Frequency 1e+6 Hz,
Temperature 200 °C
DAM; ASTM D150
 35
@Frequency 1000 Hz,
Temperature 150 °C
DAM; ASTM D150
 85
@Frequency 1000 Hz,
Temperature 175 °C
DAM; ASTM D150
 136
@Frequency 1000 Hz,
Temperature 200 °C
DAM; ASTM D150
Dielectric Strength 0.800 kV/mm
@Temperature 200 °C
DAM; Short Time; ASTM D149
 1.20 kV/mm
@Temperature 175 °C
DAM; Short Time; ASTM D149
 1.90 kV/mm
@Temperature 150 °C
DAM; Short Time; ASTM D149
 16.4 kV/mm
@Temperature 100 °C
DAM; Short Time; ASTM D149
 27.5 kV/mm
@Temperature 60.0 °C
DAM; Short Time; ASTM D149
 27.5 kV/mm
@Thickness 3.20 mm,
Temperature 23.0 °C
DAM; Short Time; ASTM D149
Dissipation Factor 0.010
@Frequency 1000 Hz,
Temperature 23.0 °C
DAM; ASTM D150
 0.010
@Frequency 1000 Hz,
Temperature 60.0 °C
DAM; ASTM D150
 0.010
@Frequency 1e+6 Hz,
Temperature 23.0 °C
DAM; ASTM D150
 0.010
@Frequency 1e+6 Hz,
Temperature 60.0 °C
DAM; ASTM D150
 0.040
@Frequency 1e+6 Hz,
Temperature 100 °C
DAM; ASTM D150
 0.10
@Frequency 1000 Hz,
Temperature 100 °C
DAM; ASTM D150
 0.15
@Frequency 1e+6 Hz,
Temperature 150 °C
DAM; ASTM D150
 0.19
@Frequency 1e+6 Hz,
Temperature 175 °C
DAM; ASTM D150
 0.39
@Frequency 1e+6 Hz,
Temperature 200 °C
DAM; ASTM D150
 0.75
@Frequency 1000 Hz,
Temperature 150 °C
DAM; ASTM D150
 0.85
@Frequency 1000 Hz,
Temperature 175 °C
DAM; ASTM D150
Comparative Tracking Index 600 V
@Temperature 23.0 °C
DAM; IEC 60112
 600 V
@Temperature 23.0 °C
DAM; UL 746A
 >= 600 V
@Temperature 23.0 °C
DAM; ASTM D3638
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 13.0 µm/m-°C
@Temperature 125 - 200 °C
DAM; ASTM E 831
 13.0 µm/m-°C
@Temperature 125 - 200 °C
DAM; ISO 11359-1/-2
 15.0 µm/m-°C
@Temperature 55.0 - 125 °C
DAM; ISO 11359-1/-2
 15.0 µm/m-°C
@Temperature 55.0 - 125 °C
DAM; ASTM E 831
 20.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 20.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ASTM E 831
 21.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ISO 11359-1/-2
 21.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ASTM E 831
CTE, linear, Transverse to Flow 57.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ASTM E 831
 57.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
DAM; ISO 11359-1/-2
 62.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ASTM E 831
 62.0 µm/m-°C
@Temperature 23.0 - 55.0 °C
DAM; ISO 11359-1/-2
 77.0 µm/m-°C
@Temperature 55.0 - 125 °C
DAM; ASTM E 831
 77.0 µm/m-°C
@Temperature 55.0 - 125 °C
DAM; ISO 11359-1/-2
 95.0 µm/m-°C
@Temperature 125 - 200 °C
DAM; ASTM E 831
 95.0 µm/m-°C
@Temperature 125 - 200 °C
DAM; ISO 11359-1/-2
Melting Point 305 °C10°C/min, First Heat; DAM; ISO 11357-1/-3
 310 °CDAM; ASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 285 °CDAM; ISO 75-1/-2
 288 °CDAM; ASTM D648
UL RTI, Electrical 150 °C
@Thickness 0.750 mm
DAM; UL 746B
 150 °C
@Thickness 3.00 mm
DAM; UL 746B
 150 °C
@Thickness 1.50 mm
DAM; UL 746B
UL RTI, Mechanical with Impact 125 °C
@Thickness 3.00 mm
DAM; UL 746B
 125 °C
@Thickness 1.50 mm
DAM; UL 746B
 125 °C
@Thickness 0.750 mm
DAM; UL 746B
UL RTI, Mechanical without Impact 130 °C
@Thickness 0.750 mm
DAM; UL 746B
 140 °C
@Thickness 1.50 mm
DAM; UL 746B
 150 °C
@Thickness 3.00 mm
DAM; UL 746B
Flammability, UL94 HB
@Thickness 0.750 mm
DAM; IEC 60695-11-10
 HB
@Thickness 0.850 mm
DAM; IEC 60695-11-10
 HB
@Thickness 3.00 mm
DAM; IEC 60695-11-10
 HB
@Thickness 1.50 mm
DAM; IEC 60695-11-10
 HB
@Thickness 0.750 mm
DAM; UL94
 HB
@Thickness 1.50 mm
DAM; UL94
 HB
@Thickness 3.00 mm
DAM; UL94
Oxygen Index 25 %DAM; ASTM D2863
 25 %DAM; ISO 4589-1/-2
Glow Wire Ignition Temperature 725 °C
@Thickness 1.50 mm
IEC 60695-2-13
 775 °C
@Thickness 0.750 mm
IEC 60695-2-13
 775 °C
@Thickness 3.00 mm
IEC 60695-2-13
Glow Wire Flammability Index 700 °C
@Thickness 1.50 mm
DAM; IEC 60695-2-12
 750 °C
@Thickness 0.750 mm
DAM; IEC 60695-2-12
 850 °C
@Thickness 3.00 mm
DAM; IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Melt Temperature 325 °CDAM; Optimum
 320 - 330 °CDAM
Mold Temperature 95.0 °CDAM; optimum
 85.0 - 105 °CDAM
Drying Temperature 100 °CDAM
Dry Time 6.00 - 8.00 hourDAM
Moisture Content <= 0.10 %DAM
 
Descriptive Properties
AdditiveHeat StabilizerDAM
 LubricantDAM
AppearanceNatural ColorDAM
Drying RecommendedYes, if moisture content of resin exceeds recommended levelDAM
FeaturesHeat Aging Resistance, GoodDAM
FillerGlass fiber reinforcementDAM
FormsPelletsDAM
GenericPolyphthalamide (PPA)DAM
Heat StabilizedYesDAM
Material StatusPreliminary DataDAM
Part Marking Code>PA6T/66-GF35<ISO 11469; DAM
 >PPA-GF35<SAE J1344; DAM
Polymer FamilyHigh performance polyamideDAM
Polymer TypePartially Aromatic PA, PPADAM
Processing MethodInjection MoldingDAM
Product CategoryGlass Reinforced ResinsDAM
Region Available - GlobalYesDAM
Resin IdentificationPA6T/66-GF35ISO 1043; DAM
Ultrasonic WeldableYesDAM
UsesAutomotive ApplicationsDAM

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Zytel® HTN 52G35HSL NC010 Polyphthalamide (PPA)
Ensinger TECASINT 1011 Polyimide (PI)
DuPont Mobility and Materials Zytel® HTN 52G35HSL NC010 Polyphthalamide (PPA) (extended Stress-Strain Tabular Data)
Celanese Zytel® HTN 51G50HSL BK083 Polyphthalamide (PPA)
Bakelite® EP 8412 Epoxy Resin, High Arc Resistance, Improved Electrical Properties, Low Shrinkage

PZDSZ1426_a / 234774

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.