MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
SABIC VALOX™ FR 4631 PBT (Europe)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: VALOX 4631 is a 30% glass filled, flame retardant Polybutylene Terephthalate (PBT) injection moldable grade. It has good electrical and mechanical properties and a UL94V0@0.75 flame rating.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.67 g/ccASTM D792
Density 1.67 g/ccISO 1183
Filler Content 30 %ASTM D229
Water Absorption 0.25 %23°C/sat; ISO 62
Moisture Absorption 0.0700 %23°C / 50% RH; ISO 62
Viscosity 115 cP
@Shear Rate 1500 1/s,
Temperature 260 °C
melt; ISO 11443
Linear Mold Shrinkage, Flow 0.0010 - 0.0030 cm/cmSABIC method
Linear Mold Shrinkage, Transverse 0.0040 - 0.0070 cm/cmSABIC method
Melt Flow 13 g/10 min
@Load 2.16 kg,
Temperature 250 °C
ASTM D1238
 40 g/10 min
@Load 5.00 kg,
Temperature 250 °C
cm³/10 min; ISO 1133
 65 g/10 min
@Load 5.00 kg,
Temperature 265 °C
cm³/10 min; ISO 1133
 67 g/10 min
@Load 5.00 kg,
Temperature 250 °C
ASTM D1238
 90 g/10 min
@Load 5.00 kg,
Temperature 266 °C
ASTM D1238
 90 g/10 min
@Load 5.00 kg,
Temperature 265 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 118ISO 2039-2
Ball Indentation Hardness 115 MPaISO 2039-1
Tensile Strength at Break 130 MPa5 mm/min; ISO 527
 130 MPa5 mm/min; ASTM D638
Tensile Strength, Yield 130 MPa5 mm/min; ISO 527
 130 MPa5 mm/min; ASTM D638
Elongation at Break 2.0 %5 mm/min; ASTM D638
 2.0 %5 mm/min; ISO 527
Elongation at Yield 2.0 %5 mm/min; ASTM D638
 2.0 %5 mm/min; ISO 527
Tensile Modulus 11500 MPa1mm/min; ISO 527
 11500 MPa5 mm/min; ASTM D638
Flexural Strength 200 MPa2 mm/min; break; ISO 178
 200 MPabrk, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Yield Strength 200 MPa2 mm/min; ISO 178
 200 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 9000 MPa1.3 mm/min, 50 mm span; ASTM D790
 9600 MPa2 mm/min; ISO 178
Flexural Strain at Break 3.0 %2 mm/min; ISO 178
Izod Impact, Notched 80.0 J/mASTM D256
 80.0 J/m
@Temperature 0.000 °C
ASTM D256
 80.0 J/m
@Temperature -30.0 °C
ASTM D256
Izod Impact, Unnotched 660 J/mASTM D4812
 660 J/m
@Temperature -30.0 °C
ASTM D4812
Izod Impact, Notched (ISO) 8.00 kJ/m²80*10*4; ISO 180/1A
 8.00 kJ/m²
@Temperature 0.000 °C
80*10*4; ISO 180/1A
 8.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 45.0 kJ/m²80*10*4; ISO 180/1U
 45.0 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1U
Charpy Impact Unnotched 50.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eU
 50.0 kJ/m²ISO 179/2C
 50.0 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
 55.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eU
Charpy Impact, Notched 10.0 kJ/m²Edgew 80*10*4 sp=62mm; ISO 179/1eA
 11.0 kJ/m²ISO 179/2C
 9.00 kJ/m²
@Temperature -30.0 °C
ISO 179/2C
 10.0 kJ/m²
@Temperature -30.0 °C
Edgew 80*10*4 sp=62mm; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity >= 1.00e+15 ohm-cmIEC 60093
 >= 1.00e+15 ohm-cmASTM D257
Surface Resistance >= 1.00e+15 ohmROA; IEC 60093
Dielectric Constant 3.0
@Frequency 50.0 - 60.0 Hz
IEC 60250
 3.5
@Frequency 1e+6 Hz
ASTM D150
 3.5
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 19.0 kV/mm
@Thickness 3.20 mm
in oil; IEC 60243-1
 23.0 kV/mm
@Thickness 1.60 mm
in oil; IEC 60243-1
 27.0 kV/mm
@Thickness 0.800 mm
in oil; IEC 60243-1
Dissipation Factor 0.0010
@Frequency 50.0 - 60.0 Hz
IEC 60250
 0.010
@Frequency 1e+6 Hz
IEC 60250
 0.010
@Frequency 1e+6 Hz
ASTM D150
Comparative Tracking Index 250 VIEC 60112
 250 - 400 VUL 746A
Hot Wire Ignition, HWI >= 120 secUL 746A
High Amp Arc Ignition, HAI 15 - 30 arcsUL 746A
High Voltage Arc-Tracking Rate, HVTR >= 150 mm/minUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 14.0 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
 16.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 21.8 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 81.8 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
 120 µm/m-°C
@Temperature 23.0 - 80.0 °C
ISO 11359-2
 130 µm/m-°C
@Temperature 23.0 - 150 °C
ISO 11359-2
Hot Ball Pressure Test 125 °CIEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi) 220 °CEdgew 120*10*4 sp=100mm; ISO 75/Be
 220 °CFlatw 80*10*4 sp=64mm; ISO 75/Bf
 220 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 205 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 205 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 205 °CRate B/50; ISO 306
 205 °CRate B/120; ISO 306
 205 °CRate B/50; ASTM D1525
 220 °CRate A/50; ASTM D1525
 220 °CRate A/50; ISO 306
UL RTI, Electrical 130 °CUL 746B
UL RTI, Mechanical with Impact 130 °CUL 746B
UL RTI, Mechanical without Impact 140 °CUL 746B
Flammability, UL94 V-0
@Thickness 0.750 mm
UL 94
Oxygen Index 34 %ISO 4589
Glow Wire Test 960 °C
@Thickness 3.00 mm
IEC 60695-2-12
 
Processing PropertiesOriginal ValueComments
Processing Temperature 40.0 - 60.0 °CHopper Temperature
Nozzle Temperature 240 - 260 °CInjection Molding
Zone 1 230 - 245 °C
Zone 2 240 - 255 °C
Zone 3 245 - 265 °C
Melt Temperature 250 - 270 °C
Mold Temperature 40.0 - 100 °C
Drying Temperature 110 - 120 °CInjection Molding
Dry Time 2.00 - 4.00 hourInjection Molding
Moisture Content 0.020 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10333 / 243800

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.