MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPV X18035 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV X18035 is a high performance thermoplastic vulcanizate used in automotive and industrial applications. This product is a low hardness, low density grade exhibiting superior compression set and chemical resistance. This grade can be processed by injection molding and extrusion.

Availability: Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; General Purpose; Good Adhesion; Good Flexibility; Good Moldability; High Elasticity; Low Density; Low Hardness; Resilient

Uses: Automotive Applications; Automotive Interior Parts; Automotive Under the Hood: Diaphragms; Gaskets; General Purpose; Industrial Applications; O-rings; Plugs; Profiles; Rubber Replacement; Seals; Weatherstirpping

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding; Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.930 g/ccISO 1183
Viscosity 270 cP
@Shear Rate 206 1/s,
Temperature 200 °C
Apparent; ASTM D3835
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 38
@Time 5.00 sec
Extruded; ISO 868
 43
@Time 5.00 sec
Injection Molded; ISO 868
Tensile Strength at Break 319 psiFlow; ISO 37
 580 psiAcross Flow; ISO 37
 580 psi
@Treatment Temp. 135 °C,
Time 3.629e+6 sec
Across Flow, Change in Air; ISO 188
 603 psi
@Treatment Temp. 150 °C,
Time 605000 sec
Across Flow, Change in Air; ISO 188
Tensile Stress at Strain 160 psi
@Strain 100 %
Across Flow; ISO 37
 305 psi
@Strain 100 %
Flow; ISO 37
 166 psi
@Strain 100 %,
Treatment Temp. 135 °C
Across Flow, Change in Air at 1008 hr; ISO 188
 178 psi
@Strain 100 %,
Treatment Temp. 150 °C
Across Flow, Change in Air at 168 hr; ISO 188
Elongation at Break 200 %Flow; ISO 37
 600 %Across Flow; ISO 37
 588 %
@Treatment Temp. 135 °C,
Time 3.629e+6 sec
Across Flow, Change in Air; ISO 188
 606 %
@Treatment Temp. 150 °C,
Time 605000 sec
Across Flow, Change in Air; ISO 188
Tear Strength 86.0 pliMethod Ba, Angle (Unnicked), Across Flow; ISO 34-1
Compression Set 15 %
@Temperature 22.8 °C,
Time 79200 sec
ISO 815
 30 %
@Temperature 70.0 °C,
Time 79200 sec
ISO 815
 52 %
@Temperature 125 °C,
Time 252000 sec
ISO 815
 
Processing PropertiesOriginal ValueComments
Processing Temperature 365 - 428 °FMelt, Injection
Rear Barrel Temperature 347 - 419 °FInjection
Middle Barrel Temperature 347 - 419 °FInjection
Front Barrel Temperature 347 - 419 °FInjection
Nozzle Temperature 365 - 428 °FInjection
Zone 1 356 - 392 °FExtrusion
Zone 2 356 - 392 °FExtrusion
Zone 3 374 - 410 °FExtrusion
Zone 4 374 - 428 °FExtrusion
Die Temperature 374 - 428 °FExtrusion
Melt Temperature 374 - 428 °FExtrusion
Mold Temperature 50.0 - 140 °FInjection
Drying Temperature 176 °F
Dry Time 3.00 hour
 
Descriptive Properties
AppearanceBlack
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
E-Polymers EFLEX® V2045 SEBS/TPV
Chengdu Polyster 4502 High Performance Grade TPV
Barlog Plastics KEBAFLEX E 50.1 TPE-V, Shore A50
Barlog Plastics KEBAFLEX E 45.1 TPE-V, Shore A45
Barlog Plastics KEBAFLEX E 40.1 TPE-V, Shore A40

PTEKNQ1231 / 237722

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.