MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Arlon Electronic Materials 44N Multifunctional Microdispersed Ceramic Filled Epoxy-Fiberglass Prepreg
Categories: Polymer; Thermoset; Epoxy

Material Notes: Arlon 44N is a high resin content multifunctional (175°C) epoxy prepreg system with a proprietary microdispersed ceramic filler system. 44N is engineered for the filling of clearance holes in thin metal cores such as 0.006" Copper-invar-Copper or via holes in sequentially laminated MLB designs. Based on Arlon's 45N, the 44N system is compatible with conventional epoxy lamination fabrication.

  • Microdisperse ceramic filled to minimize resin shrinkage and cracking in filled clearance holes
  • Prepreg format eliminated the need for messy plate fill material in high volume applications
  • High Tg compatible with conventional multifunctional epoxy processing
  • Filled system has reduced Z-direction expansion and improved thermal conductivity for improved plated through hole reliability
  • Suitable for most lead-free applications
  • RoHS/WEEE compliant

Typical Applications:

  • Automotive Under-hood applications
  • Backplanes and Mother Boards
  • Ball Grid Array Packaging
  • High layer count MLBs

    Information provided by ARLON Electronic Materials.

  • Vendors: Arlon Materials for Electronics (MED) is a major manufacturer of specialty high performance laminate and prepreg materials for use in a wide variety of printed circuit board (PCB) applications and in several distinctive markets.

    Click here to view all available suppliers for this material.

    Please click here if you are a supplier and would like information on how to add your listing to this material.

     
    Physical PropertiesOriginal ValueComments
    Density 1.85 g/ccASTM D792 Method A
    Water Absorption 0.10 %IPC TM-650 2.6.2.1
     
    Mechanical PropertiesOriginal ValueComments
    Modulus of Elasticity 2800 ksiIPC TM-650 2.4.18.3
    Poissons Ratio 0.15ASTM D3039
    Peel Strength 8.00 pliTo Copper (1 oz./35 micron); After Process Solutions; IPC TM-650 2.4.8
     8.00 pliTo Copper (1 oz./35 micron); After Thermal Stress; IPC TM-650 2.4.8
     8.00 pliTo Copper (1 oz./35 micron); At Elevated Temperatures; IPC TM-650 2.4.8.2
     
    Electrical PropertiesOriginal ValueComments
    Volume Resistivity 2.60e+13 ohm-cmC96/35/90; IPC TM-650 2.5.17.1
     3.30e+13 ohm-cmE24/125; IPC TM-650 2.5.17.1
    Surface Resistance 4.00e+10 ohmC96/35/90; IPC TM-650 2.5.17.1
     2.90e+13 ohmE24/125; IPC TM-650 2.5.17.1
    Dielectric Constant 4.2 - 4.6
    @Frequency 1e+6 Hz
    may vary with resin %; IPC TM-650 2.5.5.3
    Dielectric Strength 1500 V/milIPC TM-650 2.5.6.2
    Dissipation Factor 0.025
    @Frequency 1e+6 Hz
    IPC TM-650 2.5.5.3
    Arc Resistance 65 secIPC TM-650 2.5.1
     
    Thermal PropertiesOriginal ValueComments
    CTE, linear 14.0 - 16.0 µm/m-°CIPC TM-650 2.4.41
    CTE, linear, Transverse to Flow 55.0 µm/m-°Cz, below Tg; IPC TM-650 2.4.24
     200 µm/m-°Cz, above Tg; IPC TM-650 2.4.24
    Thermal Conductivity 0.300 W/m-KASTM E1461
    Glass Transition Temp, Tg 175 °CDSC; IPC TM-650 2.4.25
    Flammability, UL94 V-0
     
    Descriptive Properties
    Z-Axis Expansion (%)2.4IPC TM-650 2.4.24 (50-260°C)

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

    Users viewing this material also viewed the following:
    LKAB Minerals MicroCarb Chalk
    Epoxy Technology EPO-TEK® 930-4 Thermally Conductive Epoxy
    SPHERE ONE EXTENDOSPHERES™ FM-1 Hollow Spheres
    Crystex Composites Mykroy/Mycalex MM 800 Machining Grade Glass-bonded Mica Composite
    G-10 Fiberglass Epoxy Laminate Sheet

    PARLM9880 / 149033

    Rulon Bearings

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.