MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Aluminum 2219-T87 (Extended Creep-Rupture Data)
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 2000 Series Aluminum Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
This designation is considered the sole original alloy for this alloy family.
Composition information provided by the Aluminum Association and is not for design.

Key Words: UNS A92219; ISO AlCu6Mn; Aluminium 2219-T87; AA2219-T87
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.84 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 130500 kg load with 10 mm ball
Hardness, Knoop 163Converted from Brinell Hardness Value
Hardness, Rockwell A 49.5Converted from Brinell Hardness Value
Hardness, Rockwell B 80Converted from Brinell Hardness Value
Hardness, Vickers 149Converted from Brinell Hardness Value
Tensile Strength, Ultimate 69.0 ksiAA; Typical
 >= 420 MPa
@Thickness 101.6 - 127 mm
Sheet and plate
 >= 425 MPa
@Thickness 76.23 - 102 mm
Sheet and plate
 >= 440 MPa
@Thickness 0.508 - 6.32 mm
Sheet and plate
 >= 440 MPa
@Thickness 6.35 - 76.2 mm
Sheet and plate
Tensile Strength, Yield 57.0 ksiAA; Typical
 >= 340 MPa
@Thickness 101.6 - 127 mm
Sheet and plate
 >= 345 MPa
@Thickness 76.23 - 102 mm
Sheet and plate
 >= 350 MPa
@Thickness 6.35 - 76.2 mm
Sheet and plate
 >= 360 MPa
@Thickness 0.508 - 6.32 mm
Sheet and plate
Elongation at Break 3.0 %
@Thickness 101.6 - 127 mm
Sheet and plate
 4.0 %
@Thickness 76.23 - 102 mm
Sheet and plate
 5.0 - 6.0 %
@Thickness 0.508 - 6.32 mm
Sheet and plate
 6.0 - 7.0 %
@Thickness 6.35 - 76.2 mm
Sheet and plate
 10 %
@Thickness 1.59 mm
AA; Typical
Creep Strength 6.00 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
0.1% creep
 8.00 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
0.2% creep
 8.00 MPa
@Temperature 370 °C,
Time 360000 sec
0.1% creep
 11.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
0.5% creep
 11.0 MPa
@Temperature 370 °C,
Time 360000 sec
0.2% creep
 12.0 MPa
@Temperature 370 °C,
Time 36000 sec
0.1% creep
 13.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
1% creep
 17.0 MPa
@Temperature 370 °C,
Time 360000 sec
0.5% creep
 17.0 MPa
@Temperature 370 °C,
Time 36000 sec
0.2% creep
 18.0 MPa
@Temperature 370 °C,
Time 3600 sec
0.1% creep
 20.0 MPa
@Temperature 370 °C,
Time 360000 sec
1% creep
 23.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
0.1% creep
 26.0 MPa
@Temperature 370 °C,
Time 36000 sec
0.5% creep
 26.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
0.2% creep
 28.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
0.5% creep
 30.0 MPa
@Temperature 370 °C,
Time 36000 sec
1% creep
 31.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
1% creep
 32.0 MPa
@Temperature 370 °C,
Time 3600 sec
0.2% creep
 34.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.1% creep
 34.0 MPa
@Temperature 370 °C,
Time 360 sec
0.1% creep
 41.0 MPa
@Temperature 370 °C,
Time 3600 sec
0.5% creep
 45.0 MPa
@Temperature 370 °C,
Time 3600 sec
1% creep
 45.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.2% creep
 48.0 MPa
@Temperature 370 °C,
Time 360 sec
0.2% creep
 52.0 MPa
@Temperature 315 °C,
Time 360000 sec
0.5% creep
 52.0 MPa
@Temperature 370 °C,
Time 360 sec
0.5% creep
 52.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.1% creep
 55.0 MPa
@Temperature 315 °C,
Time 360000 sec
1% creep
 55.0 MPa
@Temperature 370 °C,
Time 360 sec
1% creep
 59.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
0.1% creep
 62.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.2% creep
 66.0 MPa
@Temperature 315 °C,
Time 3600 sec
0.1% creep
 69.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
0.2% creep
 69.0 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
0.1% creep
 69.0 MPa
@Temperature 260 °C,
Time 360000 sec
0.1% creep
 76.0 MPa
@Temperature 315 °C,
Time 36000 sec
0.5% creep
 83.0 MPa
@Temperature 315 °C,
Time 360 sec
0.1% creep
 83.0 MPa
@Temperature 315 °C,
Time 36000 sec
1% creep
 83.0 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
0.2% creep
 83.0 MPa
@Temperature 315 °C,
Time 3600 sec
0.2% creep
 83.0 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.1% creep
 83.0 MPa
@Temperature 230 °C,
Time 360000 sec
0.1% creep
 83.0 MPa
@Temperature 260 °C,
Time 36000 sec
0.1% creep
 90.0 MPa
@Temperature 260 °C,
Time 360000 sec
0.2% creep
 97.0 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
0.5% creep
 97.0 MPa
@Temperature 315 °C,
Time 3600 sec
0.5% creep
 97.0 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.2% creep
 97.0 MPa
@Temperature 315 °C,
Time 360 sec
0.2% creep
 97.0 MPa
@Temperature 205 °C,
Time 360000 sec
0.1% creep
 97.0 MPa
@Temperature 230 °C,
Time 36000 sec
0.1% creep
 105 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
1% creep
 105 MPa
@Temperature 315 °C,
Time 3600 sec
1% creep
 105 MPa
@Temperature 315 °C,
Time 360 sec
0.5% creep
 105 MPa
@Temperature 230 °C,
Time 360000 sec
0.2% creep
 105 MPa
@Temperature 260 °C,
Time 36000 sec
0.2% creep
 105 MPa
@Temperature 260 °C,
Time 3600 sec
0.1% creep
 110 MPa
@Temperature 315 °C,
Time 360 sec
1% creep
 110 MPa
@Temperature 260 °C,
Time 360000 sec
0.5% creep
 110 MPa
@Temperature 205 °C,
Time 36000 sec
0.1% creep
 115 MPa
@Temperature 260 °C,
Time 360000 sec
1% creep
 115 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
0.5% creep
 115 MPa
@Temperature 205 °C,
Time 360000 sec
0.2% creep
 115 MPa
@Temperature 230 °C,
Time 36000 sec
0.2% creep
 115 MPa
@Temperature 230 °C,
Time 3600 sec
0.1% creep
 125 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
1% creep
 125 MPa
@Temperature 230 °C,
Time 360000 sec
0.5% creep
 125 MPa
@Temperature 260 °C,
Time 36000 sec
0.5% creep
 125 MPa
@Temperature 260 °C,
Time 3600 sec
0.2% creep
 125 MPa
@Temperature 260 °C,
Time 360 sec
0.1% creep
 130 MPa
@Temperature 260 °C,
Time 36000 sec
1% creep
 130 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
0.5% creep
 140 MPa
@Temperature 230 °C,
Time 360000 sec
1% creep
 140 MPa
@Temperature 230 °C,
Time 360 sec
0.1% creep
 140 MPa
@Temperature 260 °C,
Time 3600 sec
0.5% creep
 140 MPa
@Temperature 205 °C,
Time 36000 sec
0.2% creep
 140 MPa
@Temperature 230 °C,
Time 3600 sec
0.2% creep
 140 MPa
@Temperature 260 °C,
Time 360 sec
0.2% creep
 140 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.1% creep
 140 MPa
@Temperature 205 °C,
Time 3600 sec
0.1% creep
 145 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
1% creep
 145 MPa
@Temperature 260 °C,
Time 3600 sec
1% creep
 145 MPa
@Temperature 205 °C,
Time 360000 sec
0.5% creep
 145 MPa
@Temperature 230 °C,
Time 36000 sec
0.5% creep
 150 MPa
@Temperature 260 °C,
Time 360 sec
0.5% creep
 160 MPa
@Temperature 230 °C,
Time 36000 sec
1% creep
 160 MPa
@Temperature 260 °C,
Time 360 sec
1% creep
 165 MPa
@Temperature 205 °C,
Time 360000 sec
1% creep
 165 MPa
@Temperature 230 °C,
Time 3600 sec
0.5% creep
 165 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.2% creep
 165 MPa
@Temperature 205 °C,
Time 3600 sec
0.2% creep
 165 MPa
@Temperature 230 °C,
Time 360 sec
0.2% creep
 165 MPa
@Temperature 150 °C,
Time 360000 sec
0.1% creep
 165 MPa
@Temperature 205 °C,
Time 360 sec
0.1% creep
 170 MPa
@Temperature 230 °C,
Time 3600 sec
1% creep
 170 MPa
@Temperature 205 °C,
Time 36000 sec
0.5% creep
 180 MPa
@Temperature 230 °C,
Time 360 sec
0.5% creep
 185 MPa
@Temperature 205 °C,
Time 36000 sec
1% creep
 195 MPa
@Temperature 230 °C,
Time 360 sec
1% creep
 200 MPa
@Temperature 205 °C,
Time 3600 sec
0.5% creep
 200 MPa
@Temperature 150 °C,
Time 360000 sec
0.2% creep
 200 MPa
@Temperature 205 °C,
Time 360 sec
0.2% creep
 205 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
0.5% creep
 205 MPa
@Temperature 150 °C,
Time 36000 sec
0.1% creep
 215 MPa
@Temperature 205 °C,
Time 3600 sec
1% creep
 230 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
1% creep
 230 MPa
@Temperature 205 °C,
Time 360 sec
0.5% creep
 235 MPa
@Temperature 150 °C,
Time 360000 sec
0.5% creep
 235 MPa
@Temperature 150 °C,
Time 36000 sec
0.2% creep
 240 MPa
@Temperature 205 °C,
Time 360 sec
1% creep
 240 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
0.1% creep
 240 MPa
@Temperature 150 °C,
Time 3600 sec
0.1% creep
 250 MPa
@Temperature 150 °C,
Time 360000 sec
1% creep
 260 MPa
@Temperature 150 °C,
Time 36000 sec
0.5% creep
 260 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
0.2% creep
 260 MPa
@Temperature 150 °C,
Time 3600 sec
0.2% creep
 260 MPa
@Temperature 100 °C,
Time 360000 sec
0.1% creep
 270 MPa
@Temperature 150 °C,
Time 360 sec
0.1% creep
 275 MPa
@Temperature 150 °C,
Time 36000 sec
1% creep
 290 MPa
@Temperature 150 °C,
Time 3600 sec
0.5% creep
 290 MPa
@Temperature 100 °C,
Time 360000 sec
0.2% creep
 290 MPa
@Temperature 150 °C,
Time 360 sec
0.2% creep
 290 MPa
@Temperature 100 °C,
Time 36000 sec
0.1% creep
 295 MPa
@Temperature 150 °C,
Time 3600 sec
1% creep
 295 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
0.5% creep
 305 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
1% creep
 305 MPa
@Temperature 100 °C,
Time 36000 sec
0.2% creep
 310 MPa
@Temperature 100 °C,
Time 360000 sec
0.5% creep
 310 MPa
@Temperature 150 °C,
Time 360 sec
0.5% creep
 310 MPa
@Temperature 100 °C,
Time 3600 sec
0.1% creep
 315 MPa
@Temperature 100 °C,
Time 360000 sec
1% creep
 315 MPa
@Temperature 150 °C,
Time 360 sec
1% creep
 325 MPa
@Temperature 100 °C,
Time 36000 sec
0.5% creep
 325 MPa
@Temperature 100 °C,
Time 3600 sec
0.2% creep
 325 MPa
@Temperature 100 °C,
Time 360 sec
0.1% creep
 330 MPa
@Temperature 100 °C,
Time 36000 sec
1% creep
 340 MPa
@Temperature 100 °C,
Time 3600 sec
0.5% creep
 340 MPa
@Temperature 100 °C,
Time 360 sec
0.2% creep
 345 MPa
@Temperature 100 °C,
Time 3600 sec
1% creep
 345 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
0.1% creep
 350 MPa
@Temperature 100 °C,
Time 360 sec
0.5% creep
 350 MPa
@Temperature 24.0 °C,
Time 360000 sec
0.1% creep
 360 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
0.2% creep
 360 MPa
@Temperature 24.0 °C,
Time 36000 sec
0.1% creep
 365 MPa
@Temperature 100 °C,
Time 360 sec
1% creep
 365 MPa
@Temperature 24.0 °C,
Time 360000 sec
0.2% creep
 365 MPa
@Temperature 24.0 °C,
Time 3600 sec
0.1% creep
 370 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
0.5% creep
 370 MPa
@Temperature 24.0 °C,
Time 36000 sec
0.2% creep
 370 MPa
@Temperature 24.0 °C,
Time 360 sec
0.1% creep
 380 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
1% creep
 380 MPa
@Temperature 24.0 °C,
Time 360000 sec
0.5% creep
 380 MPa
@Temperature 24.0 °C,
Time 3600 sec
0.2% creep
 385 MPa
@Temperature 24.0 °C,
Time 36000 sec
0.5% creep
 385 MPa
@Temperature 24.0 °C,
Time 360 sec
0.2% creep
 395 MPa
@Temperature 24.0 °C,
Time 360000 sec
1% creep
 400 MPa
@Temperature 24.0 °C,
Time 3600 sec
0.5% creep
 405 MPa
@Temperature 24.0 °C,
Time 36000 sec
1% creep
 420 MPa
@Temperature 24.0 °C,
Time 360 sec
0.5% creep
 425 MPa
@Temperature 24.0 °C,
Time 3600 sec
1% creep
 450 MPa
@Temperature 24.0 °C,
Time 360 sec
1% creep
Rupture Strength 17.0 MPa
@Temperature 370 °C,
Time 3.60e+6 sec
 23.0 MPa
@Temperature 370 °C,
Time 360000 sec
 34.0 MPa
@Temperature 315 °C,
Time 3.60e+6 sec
 34.0 MPa
@Temperature 370 °C,
Time 36000 sec
 48.0 MPa
@Temperature 370 °C,
Time 3600 sec
 59.0 MPa
@Temperature 370 °C,
Time 360 sec
 62.0 MPa
@Temperature 315 °C,
Time 360000 sec
 90.0 MPa
@Temperature 315 °C,
Time 36000 sec
 105 MPa
@Temperature 260 °C,
Time 3.60e+6 sec
 105 MPa
@Temperature 315 °C,
Time 3600 sec
 115 MPa
@Temperature 315 °C,
Time 360 sec
 125 MPa
@Temperature 260 °C,
Time 360000 sec
 145 MPa
@Temperature 260 °C,
Time 36000 sec
 150 MPa
@Temperature 205 °C,
Time 3.60e+6 sec
 150 MPa
@Temperature 230 °C,
Time 360000 sec
 160 MPa
@Temperature 260 °C,
Time 3600 sec
 170 MPa
@Temperature 230 °C,
Time 36000 sec
 170 MPa
@Temperature 260 °C,
Time 360 sec
 180 MPa
@Temperature 205 °C,
Time 360000 sec
 185 MPa
@Temperature 230 °C,
Time 3600 sec
 205 MPa
@Temperature 205 °C,
Time 36000 sec
 206 MPa
@Temperature 230 °C,
Time 360 sec
 230 MPa
@Temperature 205 °C,
Time 3600 sec
 235 MPa
@Temperature 150 °C,
Time 3.60e+6 sec
 255 MPa
@Temperature 205 °C,
Time 360 sec
 260 MPa
@Temperature 150 °C,
Time 360000 sec
 290 MPa
@Temperature 150 °C,
Time 36000 sec
 315 MPa
@Temperature 100 °C,
Time 3.60e+6 sec
 315 MPa
@Temperature 150 °C,
Time 3600 sec
 330 MPa
@Temperature 100 °C,
Time 360000 sec
 345 MPa
@Temperature 150 °C,
Time 360 sec
 350 MPa
@Temperature 100 °C,
Time 36000 sec
 380 MPa
@Temperature 100 °C,
Time 3600 sec
 400 MPa
@Temperature 100 °C,
Time 360 sec
 420 MPa
@Temperature 24.0 °C,
Time 3.60e+6 sec
 435 MPa
@Temperature 24.0 °C,
Time 360000 sec
 450 MPa
@Temperature 24.0 °C,
Time 36000 sec
 455 MPa
@Temperature 24.0 °C,
Time 3600 sec
 460 MPa
@Temperature 24.0 °C,
Time 360 sec
 1130 MPa
@Temperature 230 °C,
Time 3.60e+6 sec
Modulus of Elasticity 10600 ksiAA; Typical; Average of tension and compression. Compression modulus is about 2% greater than tensile modulus.
Notched Tensile Strength 379 MPa2.5 cm width x 0.16 cm thick side-notched specimen, Kt = 17.
Poissons Ratio 0.33Estimated from trends in similar Al alloys.
Fatigue Strength 15000 psi
@# of Cycles 5.00e+8
completely reversed stress; RR Moore machine/specimen
Shear Modulus 27.0 GPaEstimated from similar Al alloys.
Shear Strength 280 MPa
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 35.0 ohm-cir-mil/ft
@Temperature 20.0 °C
AA; Typical
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.4 µin/in-°F
@Temperature 20.0 - 100 °C
AA; Typical; average over range
 20.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 22.5 µm/m-°C
@Temperature 20.0 - 100 °C
 23.4 µm/m-°C
@Temperature 20.0 - 200 °C
 24.1 µm/m-°C
@Temperature 20.0 - 300 °C
 24.4 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.864 J/g-°C
Thermal Conductivity 840 BTU-in/hr-ft²-°FAA; Typical at 77°F
Melting Point 1010 - 1190 °FAA; Typical range based on typical composition for wrought products >= 1/4 in. thickness. Eutectic melting is not eliminated by homogenization.
Solidus 1010 °FAA; Typical
Liquidus 1190 °FAA; Typical
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 775 °F
Solution Temperature 995 °F
Aging Temperature 325 - 375 °Ffrom 18 to 36 hr at temperature
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 91.5 - 93.8 %As remainder
Copper, Cu 5.8 - 6.8 %
Iron, Fe <= 0.30 %
Magnesium, Mg <= 0.02 %
Manganese, Mn 0.20 - 0.40 %
Other, each <= 0.05 %
Other, total <= 0.15 %
Silicon, Si <= 0.20 %
Titanium, Ti 0.02 - 0.10 %
Vanadium, V 0.05 - 0.15 %
Zinc, Zn <= 0.10 %
Zirconium, Zr 0.10 - 0.25 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 2618-T61 (Includes Creep/Rupture Data)
Aluminum 7178-T6; 7178-T651 (Included Creep/Rupture Data)
AISI 8620H Steel, quenched from 900°C (1650°F), tempered at 650°C (1200°F), Low temp impact properties
Aluminum 6069-T6, Cold Impact Extruded Cylinder, Minimum Tensile Values
Aluminum 2218-T61 (Includes Creep/Rupture/Fatigue Data)

MA2219T87a / 170644

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.