MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Kennametal Stellite Stellite® 6B solution heat-treated at 1232°C, 1.6 mm thick sheet
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Superalloy

Material Notes: Machined with tungsten-carbide tools. Inherent wear resistance, resistant to the wearing effects of hard, sharp particles such as in screw conveyors, rock crushing rollers, tile-making machines, and cement and steel-mill equipment. Resistant to the effects of seizing or galling, low coefficient of friction alloys sliding contact with other metals. Used in equipment where no lubricants are used. Outstanding resistance to cavitation-erosion. Combines wear and corrosion resistance with good impact strength and resistance to thermal shock. Retains high hardness, even at red heat. Electrical conductivity 1.90% compared to Copper. 2360 MPa average modulus of rupture of sheet at room temperature. Data provided by the manufacturer, Deloro Stellite, Inc.

Product of former Deloro Stellite Inc.

Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.387 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 102
@Temperature 871 °C
Mutual indentation method
 167
@Temperature 760 °C
Mutual indentation method
 203
@Temperature 649 °C
Mutual indentation method
 226
@Temperature 538 °C
Mutual indentation method
Hardness, Knoop 117
@Temperature 871 °C
Converted from Brinell Hardnesses
 194
@Temperature 760 °C
Converted from Brinell Hardnesses
 237
@Temperature 649 °C
Converted from Brinell Hardnesses
 265
@Temperature 538 °C
Converted from Brinell Hardnesses
Hardness, Rockwell A 36
@Temperature 871 °C
Converted from Brinell Hardnesses
 52
@Temperature 760 °C
Converted from Brinell Hardnesses
 58
@Temperature 649 °C
Converted from Brinell Hardnesses
 60
@Temperature 538 °C
Converted from Brinell Hardnesses
Hardness, Rockwell B 55
@Temperature 871 °C
Converted from Brinell Hardnesses
 86
@Temperature 760 °C
Converted from Brinell Hardnesses
 94
@Temperature 649 °C
Converted from Brinell Hardnesses
 98
@Temperature 538 °C
Converted from Brinell Hardnesses
Hardness, Vickers 102
@Temperature 871 °C
Converted from Brinell Hardnesses
 170
@Temperature 760 °C
Converted from Brinell Hardnesses
 208
@Temperature 649 °C
Converted from Brinell Hardnesses
 232
@Temperature 538 °C
Converted from Brinell Hardnesses
Tensile Strength, Ultimate 1007 MPa
 92.0 MPa
@Temperature 1150 °C
 134 MPa
@Temperature 1090 °C
 225 MPa
@Temperature 982 °C
 385 MPa
@Temperature 871 °C
 509 MPa
@Temperature 816 °C
Tensile Strength, Yield 632 MPa
@Strain 0.2 %
 53.0 MPa
@Strain 0.2 %,
Temperature 1150 °C
 75.0 MPa
@Strain 0.2 %,
Temperature 1090 °C
 137 MPa
@Strain 0.2 %,
Temperature 982 °C
 270 MPa
@Strain 0.2 %,
Temperature 871 °C
 313 MPa
@Strain 0.2 %,
Temperature 816 °C
Elongation at Break 11 %in 50.8 mm
 17 %
@Temperature 816 °C
in 50.8 mm
 18 %
@Temperature 871 °C
in 50.8 mm
 22 %
@Temperature 1150 °C
in 50.8 mm
 36 %
@Temperature 982 °C
in 50.8 mm
 44 %
@Temperature 1090 °C
in 50.8 mm
Modulus of Elasticity 214 GPasheet at RT
 210 GPa
@Diameter 15.9 mm,
Temperature 23.0 °C
bar
Izod Impact Unnotched 84.0 J
@Thickness 12.7 mm
plate, solution heat-treated at 1232°C (2250°F), air cooled, tested at RT.
Charpy Impact 8.00 J
@Temperature 23.0 °C
Longitudinal
 20.0 J
@Temperature 538 - 816 °C
Longitudinal
Charpy Impact, Unnotched 88.0 JTransverse
 98.0 J
@Temperature 22.2 °C
Longitudinal
 110 J
@Temperature 538 °C
Longitudinal
 157 J
@Temperature 677 °C
Longitudinal
 171 J
@Temperature 816 °C
Longitudinal
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000910 ohm-cm
@Temperature 22.0 °C
Magnetic Permeability <= 1.2
@Temperature 22.0 °C
200 Oersted (15.900 A/m)
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.9 µm/m-°C
@Temperature 0.000 - 100 °C
 14.1 µm/m-°C
@Temperature 0.000 - 200 °C
 14.5 µm/m-°C
@Temperature 0.000 - 300 °C
 14.7 µm/m-°C
@Temperature 0.000 - 400 °C
 15.0 µm/m-°C
@Temperature 0.000 - 500 °C
 15.3 µm/m-°C
@Temperature 0.000 - 600 °C
 15.8 µm/m-°C
@Temperature 0.000 - 700 °C
 16.3 µm/m-°C
@Temperature 0.000 - 800 °C
 16.9 µm/m-°C
@Temperature 0.000 - 900 °C
 17.4 µm/m-°C
@Temperature 0.000 - 1000 °C
Specific Heat Capacity 0.423 J/g-°Cat RT (calculated)
Thermal Conductivity 14.85 W/m-K
Melting Point 1265 - 1354 °C
Solidus 1265 °C
Liquidus 1354 °C
 
Optical PropertiesOriginal ValueComments
Reflection Coefficient, Visible (0-1) 0.57 - 0.70reflecting power
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.90 - 1.4 %
Chromium, Cr 28 - 32 %
Cobalt, Co 50 - 67 %As remainder
Iron, Fe <= 3.0 %
Manganese, Mn <= 2.0 %
Molybdenum, Mo <= 1.5 %
Nickel, Ni <= 3.0 %
Silicon, Si <= 2.0 %
Tungsten, W 3.5 - 5.5 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Kennametal Stellite Stellite® 6B solution heat-treated at 1232°C, air cooled, 1.7 mm thick sheet
Kennametal Stellite Stellite® 6B solution heat-treated at 1232°C, air cooled, 11.1 mm thick plate
Kennametal Stellite Stellite® 6B solution heat-treated at 1232°C, air cooled, 15.9 mm thick plate
Kennametal Stellite Stellite® 6B solution heat-treated at 1232°C, air cooled, 3.2 mm thick sheet
Kennametal Stellite Stellite® 6B solution heat-treated at 1232°C, air cooled, 4.8 mm thick sheet

NST6BK / 19220

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.