MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Teknor Apex Medalist® MD-10308 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Medalist MD-10308 is a high performance thermoplastic elastomer specifically designed for healthcare and medical applications. Medalist MD-10308 is a low hardness, low density, halogen-free grade that can be sterilized and is suitable for injection molding, extrusion and cast film.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Chemical Resistant; Ethylene Oxide Sterilizable; Good Adhesion; Good Colorability; Good Melt Strength; Good Processability; Good Stretchability; good Toughness; Halogen Free; High Clarity; High Elasticity; High Elongation; Low Density; Low Hardness; Low Odor; Low Specific Gravity; Puncture Resistant; Resilient; Soft

Uses: Dental Applications; Film; Hospital Goods; Medical Devices; Medical/Healthcare Applications; Rubber Replacement

Agency Ratings: ISO 10993 Part 5; ISO 13485

Form: Pellets

Processing Method: Injection Molding; Film Extrusion; Cast Film

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.870 g/ccASTM D792
Melt Flow 15 g/10 min
@Load 2.16 kg,
Temperature 190 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 8.0
@Time 5.00 sec
Injection Molded; ASTM D2240
 10
@Time 1.00 sec
Injection Molded; ASTM D2240
Tensile Strength at Break 615 psiDie C, 20 in/min; ASTM D412
Tensile Stress at Strain 30.0 psi
@Strain 100 %
Die C, 20 in/min; ASTM D412
 60.0 psi
@Strain 300 %
Die C, 20 in/min; ASTM D412
Elongation at Break 800 %Die C, 20 in/min; ASTM D412
Tear Strength 90.0 pliDie C, 20 in/min; ASTM D624
Compression Set 11 %
@Temperature 22.8 °C,
Time 86400 sec
Type 1; ASTM D395B
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature <= -76.0 °FASTM D746
 
Processing PropertiesOriginal ValueComments
Processing Temperature 365 - 392 °FMelt, Injection
Rear Barrel Temperature 338 - 356 °FInjection
Middle Barrel Temperature 365 - 392 °FInjection
Front Barrel Temperature 365 - 392 °FInjection
Nozzle Temperature 365 - 392 °FInjection
Zone 1 370 - 400 °FExtrusion
Zone 2 385 - 405 °FExtrusion
Zone 3 390 - 410 °FExtrusion
Zone 4 390 - 410 °FExtrusion
Zone 5 400 - 420 °FExtrusion
Die Temperature 400 - 420 °FExtrusion
Mold Temperature 50.0 - 100 °FInjection
Cushion 0.140 - 1.00 inInjection
Screw Speed 30 - 100 rpmExtrusion
 50 - 100 rpmInjection
 
Descriptive Properties
AppearanceClear/Transparent
 Colors Available

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Teknor Apex Medalist® MD-100 Thermoplastic Elastomer
Teknor Apex Medalist® MD-50133 Thermoplastic Elastomer
Teknor Apex Medalist® MD-23115 Thermoplastic Vulcanizate Elastomer
Teknor Apex Medalist® MD-200 Thermoplastic Elastomer
Teknor Apex Medalist® MD-16376 X Thermoplastic Elastomer

PTEKNQ0678 / 237169

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.