MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Corning ULE® 7972 Ultra Low Expansion Glass
Categories: Ceramic; Glass; Optical

Material Notes: ULE® Corning Code 7972 Ultra Low Expansion Glass is a titania silicate glass. It is used in applications ranging from machine tool reference blocks to solid and lightweight mirror blanks for large astronomical telescopes and space satellite applications. The mean linear CTE is 0 ± 30 ppb/°C from 5°C to 35°C with a 95% confidence level, and is tested on each boule.

Excellent resistance to weathering. Exhibits virtually no surface clouding or electrical surface leakage when subjected to attack by water, sulfur dioxide, and other atmospheric gases. High resistance to attack by nearly all chemical agents.

Information provided by Corning Incorporated.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.21 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Knoop 460kg/mm² at 200g load
Tensile Strength, Ultimate 49.8 MPa
Modulus of Elasticity 67.6 GPa
Bulk Modulus 34.1 GPa
Poissons Ratio 0.17
Shear Modulus 29.0 GPa
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 4.00e+11 ohm-cm
@Temperature 200 °C
100Hz
 
Thermal PropertiesOriginal ValueComments
CTE, linear -0.390 µm/m-°C
@Temperature -100 °C
Approximate Instantaneous Value
 -0.180 µm/m-°C
@Temperature -50.0 °C
Approximate Instantaneous Value
 -0.0500 µm/m-°C
@Temperature 0.000 °C
Approximate Instantaneous Value
 -0.0300 - 0.0300 µm/m-°C
@Temperature 5.00 - 35.0 °C
Specified mean from 5 to 35°C
 0.0400 µm/m-°C
@Temperature 150 °C
Approximate Instantaneous Value
 0.0500 µm/m-°C
@Temperature 50.0 °C
Approximate Instantaneous Value
 0.0700 µm/m-°C
@Temperature 100 °C
Approximate Instantaneous Value
Specific Heat Capacity 0.767 J/g-°C
@Temperature 25.0 °C
Thermal Conductivity 1.31 W/m-K
@Temperature 25.0 °C
Softening Point 1490 °C
Annealing Point 1000 °C
Strain Point 890 °C
 
Optical PropertiesOriginal ValueComments
Refractive Index 1.4801
@Wavelength 656 nm
nC
 1.4828
@Wavelength 589 nm
nD
 1.4892
@Wavelength 486 nm
nF
Abbe Number 53.1vd
 
Descriptive Properties
Stress Optical Coefficient4.15 (nm/cm)/(kg/cm²)
Thermal Diffusivity.0079 cm²/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
CeramTec Sikor® S Cordierite
CeramTec Sikor® E Cordierite
Aluminum 6082-T6
Aluminum 6063-T5
Schott ZERODUR® Glass Ceramic

CCORNG970 / 233285

Ensinger PEI

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.