MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
SABIC VALOX™ K4530 PBT (Americas)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT)

Material Notes: 15% glass reinforced PBT, Hydrolytically stable, High flow, Automotive connectors.

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.41 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0070 - 0.0090 cm/cm
@Thickness 3.20 mm
SABIC method
Linear Mold Shrinkage, Transverse 0.010 - 0.012 cm/cm
@Thickness 3.20 mm
SABIC method
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 82.0 MPa5 mm/min; AFTER 40 CYCLES, SIMILAR TO USCAR-2, CLASS III; ASTM D638
 89.0 MPa5 mm/min; AFTER 40 CYCLES, SIMILAR TO USCAR-2, CLASS IV; ASTM D638
 98.0 MPa5 mm/min; PROPERTIES AFTER 1008 HOURS AT 125°C; ASTM D638
 103 MPa5 mm/min; ASTM D638
Tensile Strength, Yield 103 MPa5 mm/min; ASTM D638
Elongation at Break 2.3 %5 mm/min; ASTM D638
 2.5 %5 mm/min; ASTM D638
 4.0 %5 mm/min; ASTM D638
 4.0 %5 mm/min; ASTM D638
Elongation at Yield 4.0 %5 mm/min; ASTM D638
 97.2 %5 mm/min; PROPERTIES AFTER 1008 HOURS AT 155°C; ASTM D638
Tensile Modulus 3550 MPa5 mm/min; ASTM D638
Flexural Strength 150 MPabrk, 1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 4520 MPa1.3 mm/min, 50 mm span; AFTER 40 CYCLES, SIMILAR TO USCAR-2, CLASS III; ASTM D790
 4640 MPa1.3 mm/min, 50 mm span; ASTM D790
 4820 MPa1.3 mm/min, 50 mm span; PROPERTIES AFTER 1008 HOURS AT 125°C; ASTM D790
 5100 MPa1.3 mm/min, 50 mm span; AFTER 40 CYCLES, SIMILAR TO USCAR-2, CLASS IV; ASTM D790
Flexural Strain at Yield 3.8 %1.3 mm/min, 50 mm span; ASTM D790
 6.0 %1.3 mm/min, 50 mm span; ASTM D790
 7.0 %1.3 mm/min, 50 mm span; ASTM D790
 9.7 %1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 58.0 J/mASTM D256
Izod Impact, Unnotched 400 J/mASTM D4812
Dart Drop, Total Energy 4.00 JAFTER 40 CYCLES, SIMILAR TO USCAR-2, CLASS IV; ASTM D3763
 5.00 JPROPERTIES AFTER 1008 HOURS AT 125°C; ASTM D3763
 6.00 JAFTER 40 CYCLES, SIMILAR TO USCAR-2, CLASS III; ASTM D3763
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 218 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 193 °C
@Thickness 3.20 mm
unannealed; ASTM D648
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 245 - 260 °CInjection Molding
Zone 1 240 - 255 °C
Zone 2 245 - 260 °C
Zone 3 250 - 265 °C
Melt Temperature 250 - 265 °C
Mold Temperature 65.0 - 90.0 °C
Drying Temperature 60.0 - 75.0 °CInjection Molding
Dry Time 4.00 - 6.00 hourInjection Molding
 8.00 hourCumulative; Injection Molding
Moisture Content 0.050 %
Back Pressure 0.300 - 0.700 MPa
Shot Size 40 - 80 %
Vent Depth 0.00250 - 0.00380 cm
Screw Speed 50 - 80 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10281 / 243748

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.