Physical Properties | Original Value | Comments |
---|
Specific Gravity | 1.84 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Hardness, Shore A | 75 |
| 64 @Temperature 200 °C, Time 252000 sec |
| 69 @Temperature 200 °C, Time 252000 sec |
| 73 @Temperature 23.0 °C, Time 252000 sec |
| 75 @Temperature 150 °C, Time 252000 sec |
| 75 @Temperature 150 °C, Time 252000 sec |
| 75 @Temperature 100 °C, Time 252000 sec |
| 75 @Temperature 23.0 °C, Time 252000 sec |
| 75 @Temperature 23.0 °C, Time 252000 sec |
| 75 @Temperature 275 °C, Time 252000 sec |
| 75 @Temperature 250 °C, Time 252000 sec |
Tensile Strength | 2408 psi |
| 1688 psi @Temperature 200 °C, Time 252000 sec |
| 1844.5 psi @Temperature 200 °C, Time 252000 sec |
| 1895.1 psi @Temperature 275 °C, Time 252000 sec |
| 1974.6 psi @Temperature 23.0 °C, Time 252000 sec |
| 1981.8 psi @Temperature 23.0 °C, Time 252000 sec |
| 2107 psi @Temperature 150 °C, Time 252000 sec |
| 2109.4 psi @Temperature 150 °C, Time 252000 sec |
| 2229.8 psi @Temperature 250 °C, Time 252000 sec |
| 2297.2 psi @Temperature 23.0 °C, Time 252000 sec |
Elongation, Ultimate | 311 % |
| 281.1 % @Temperature 150 °C, Time 252000 sec |
| 291 % @Temperature 250 °C, Time 252000 sec |
| 292.1 % @Temperature 23.0 °C, Time 252000 sec |
| 303.8 % @Temperature 23.0 °C, Time 252000 sec |
| 314.11 % @Temperature 23.0 °C, Time 252000 sec |
| 325 % @Temperature 150 °C, Time 252000 sec |
| 329 % @Temperature 200 °C, Time 252000 sec |
| 360.1 % @Temperature 200 °C, Time 252000 sec |
| 366 % @Temperature 275 °C, Time 252000 sec |
100% Modulus | 571 psi |
Tear Strength | 167 pli |
| 194 pli |
Compression Set | 12.8 % @Temperature 175 °C, Time 79200 sec |
| 15 % @Temperature 200 °C, Time 79200 sec |
| 21 % @Temperature 23.0 °C, Time 79200 sec |
|
Thermal Properties | Original Value | Comments |
---|
Brittleness Temperature | -14.0 °F |
Shrinkage | 0.00 % @Temperature 23.0 °C, Time 252000 sec |
| 0.10 % @Temperature 150 °C, Time 252000 sec |
| 1.4 % @Temperature 150 °C, Time 252000 sec |
| 1.7 % @Temperature 23.0 °C, Time 252000 sec |
| 2.2 % @Temperature 100 °C, Time 252000 sec |
| 4.3 % @Temperature 23.0 °C, Time 252000 sec |
| 10 % @Temperature 200 °C, Time 252000 sec |
| 17.9 % @Temperature 200 °C, Time 252000 sec |
|
Descriptive Properties |
---|
Color | Black |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.