MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

(Viewing data as-entered. Click here to return)
SABIC CYCOLAC™ MG37EPX ABS (Americas)
Categories: Polymer; Thermoplastic; ABS Polymer

Material Notes: ABS plating grade optimized for a broad processing window for both painted and plated applications. NSF standard 61 compliant (80 sq in/L)

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.05 g/ccASTM D792
Density 1.05 g/ccISO 1183
Viscosity 2170 cP
@Shear Rate 1000 1/s,
Temperature 240 °C
melt; ASTM D3825
Linear Mold Shrinkage, Flow 0.0040 - 0.0060 cm/cm
@Thickness 3.20 mm
SABIC method
Melt Flow 6.6 g/10 min
@Load 3.80 kg,
Temperature 230 °C
ASTM D1238
 22 g/10 min
@Load 10.0 kg,
Temperature 220 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 106ASTM D785
Tensile Strength at Break 39.0 MPa5 mm/min; ISO 527
Tensile Strength, Yield 44.0 MPa5 mm/min; ASTM D638
 48.0 MPa5 mm/min; ISO 527
Elongation at Break 18.3 %5 mm/min; ISO 527
 54 %5 mm/min; ASTM D638
Elongation at Yield 2.0 %5 mm/min; ISO 527
Tensile Modulus 2470 MPa5 mm/min; ASTM D638
 2760 MPa1mm/min; ISO 527
Flexural Yield Strength 73.0 MPa2 mm/min; ISO 178
 90.0 MPa1.3 mm/min, 50 mm span; ASTM D790
Flexural Modulus 2470 MPa2 mm/min; ISO 178
 2810 MPa1.3 mm/min, 50 mm span; ASTM D790
Izod Impact, Notched 250 J/mASTM D256
 88.0 J/m
@Temperature -40.0 °C
ASTM D256
Izod Impact, Notched (ISO) 23.0 kJ/m²80*10*4; ISO 180/1A
 6.00 kJ/m²
@Temperature -40.0 °C
80*10*4; ISO 180/1A
 8.00 kJ/m²
@Temperature -30.0 °C
80*10*4; ISO 180/1A
Dart Drop, Total Energy 35.0 JASTM D3763
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
CTE, linear, Transverse to Flow 60.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 88.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 82.0 °CFlatw 80*10*4 sp=64mm; ISO 75/Af
 76.0 °C
@Thickness 3.20 mm
unannealed; ASTM D648
Vicat Softening Point 98.0 °CRate B/50; ISO 306
Flammability, UL94 HB
@Thickness 1.52 mm
UL 94
 
Processing PropertiesOriginal ValueComments
Nozzle Temperature 255 - 280 °CInjection Molding
Zone 1 215 - 230 °C
Zone 2 230 - 245 °C
Zone 3 250 - 270 °C
Melt Temperature 255 - 280 °C
Mold Temperature 40.0 - 80.0 °C
Drying Temperature 80.0 - 95.0 °CInjection Molding
Dry Time 2.00 - 4.00 hourInjection Molding
 8.00 hourCumulative; Injection Molding
Moisture Content 0.050 %
Back Pressure 0.300 - 0.700 MPa
Shot Size 50 - 70 %
Vent Depth 0.00380 - 0.00510 cm
Screw Speed 30 - 60 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSABI10082 / 243549

Specialty Compounds RTP Company

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.